{"id":830,"date":"2024-12-13T12:09:09","date_gmt":"2024-12-13T09:09:09","guid":{"rendered":"https:\/\/www.defencemetal.com\/test2\/?page_id=830"},"modified":"2026-09-25T16:26:25","modified_gmt":"2026-09-25T13:26:25","slug":"hastelloy-b-3","status":"publish","type":"page","link":"https:\/\/www.defencemetal.com\/index.php\/hastelloy-b-3\/","title":{"rendered":"Hastelloy B-3"},"content":{"rendered":"<p><!-- dm-hap --><\/p>\n<h1 class=\"dm-ust-baslik\" style=\"font-family:-apple-system,BlinkMacSystemFont,'Segoe UI',Helvetica,Arial,sans-serif !important;text-transform:none !important;font-size:27px;line-height:1.3;font-weight:800;color:#12303f;margin:0 0 10px;letter-spacing:-.01em;\">Hastelloy B-3 \/ (2.4600) \/ UNS N10675<\/h1>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:0 0 22px;position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"background:#12303f;padding:14px 16px 12px;position:relative;z-index:2;\">\n<div style=\"font-size:22px;font-weight:700;color:#fff;line-height:1.25;\">Hastelloy B-3<\/div>\n<div style=\"font-family:ui-monospace,Menlo,Consolas,monospace;font-size:12.5px;color:#b9cfdb;line-height:1.5;margin-top:5px;word-wrap:break-word;\">UNS N10675 \u00b7 W.Nr. 2.4600 \u00b7 NiMo29Cr (DIN 17744) \u00b7 ISO NiMo30Cr \/ Ni1067 \u00b7 Ni %65,0 min \u2013 Mo %27,0-32,0 \u2013 Cr %1,0-3,0 \u2013 Fe %1,0-3,0 \u2013 Co %3,0 maks. \u2013 Mn %3,0 maks. \u2013 W %3,0 maks. \u2013 Al %0,50 maks. \u2013 Ti %0,20 maks. \u2013 Si %0,10 maks. \u2013 C %0,010 maks. Haynes International&#8217;\u0131n verdi\u011fi nominal de\u011ferler: Ni 65, Mo 28,5, Cr 1,5, Fe 1,5. B-2 \u0130LE KARI\u015eTIRMAYIN: B-2 (UNS N10665) ayr\u0131 bir ala\u015f\u0131md\u0131r ve B-3 onun yerine ge\u00e7mek \u00fczere geli\u015ftirilmi\u015ftir (bkz. kar\u015f\u0131la\u015ft\u0131rma diyagram\u0131). Ticari adlar: HASTELLOY B-3 (Haynes International) \u00b7 Alloy B-3 (Corrosion Materials) \u00b7 Alloy B3 (Zapp, Virgamet).<\/div>\n<div data-dmkars-blok=\"1\" style=\"border-top:1px solid rgba(255,255,255,.16);margin-top:13px;padding-top:11px;\">\n<div style=\"font-size:10px;letter-spacing:.09em;text-transform:uppercase;color:#7f9fb0;font-weight:700;margin-bottom:8px;\">Kar\u0131\u015ft\u0131r\u0131lmamas\u0131 gerekenler<\/div>\n<p><a href=\"https:\/\/www.defencemetal.com\/index.php\/2026\/09\/15\/hastelloy-b-3-c-276-farki\/\" data-dmkars=\"1\" style=\"display:inline-block;padding:4px 11px;border:1px solid rgba(36,190,229,.45);background:rgba(36,190,229,.12);border-radius:99px;margin:0 6px 6px 0;font-size:12.5px;font-weight:600;color:#9fe2f7;text-decoration:none;\">Hastelloy C-276<\/a><\/div>\n<\/div>\n<div style=\"position:relative;z-index:2;\">\n<div style=\"display:flex;flex-wrap:wrap;border-top:1px solid #eceff1;\">\n<div style=\"flex:0 0 118px;padding:11px 14px;background:#F7FAFB;font-size:10.5px;letter-spacing:.09em;text-transform:uppercase;color:#6b8091;font-weight:600;line-height:1.5;\">Ne i\u00e7in<\/div>\n<div style=\"flex:1 1 230px;min-width:0;padding:11px 14px;font-size:14.5px;line-height:1.7;color:#3d5260;word-wrap:break-word;overflow-wrap:break-word;\">Ni-Mo esasl\u0131 KATI \u00c7\u00d6ZELT\u0130 ala\u015f\u0131m\u0131. \u00c7\u00d6KELME SERTLE\u015eMEZ; \u0131s\u0131l i\u015flemle sertle\u015ftirilemez, dayan\u0131m yaln\u0131zca so\u011fuk \u015fekillendirmeyle artar ve \u00e7\u00f6zelti tav\u0131 ile geri al\u0131n\u0131r.<\/div>\n<\/div>\n<div style=\"display:flex;flex-wrap:wrap;border-top:1px solid #eceff1;\">\n<div style=\"flex:0 0 118px;padding:11px 14px;background:#F7FAFB;font-size:10.5px;letter-spacing:.09em;text-transform:uppercase;color:#6b8091;font-weight:600;line-height:1.5;\">Formlar<\/div>\n<div style=\"flex:1 1 230px;min-width:0;padding:11px 14px;font-size:14.5px;line-height:1.7;color:#3d5260;word-wrap:break-word;overflow-wrap:break-word;\">Yuvarlak \u00e7ubuk \u00b7 levha \u00b7 sac \u00b7 \u015ferit \u00b7 diki\u015fsiz boru ve t\u00fcp \u00b7 diki\u015fli boru \u00b7 diki\u015fli t\u00fcp \u00b7 d\u00f6vme \u00b7 d\u00f6vme fitting \u00b7 flan\u015f \u00b7 valf g\u00f6vdesi \u00b7 \u00e7\u0131plak kaynak teli \u00b7 \u00f6rt\u00fcl\u00fc elektrot. T\u00fcm formlar sipari\u015f bazl\u0131 temin edilmektedir.<\/div>\n<\/div>\n<div style=\"display:flex;flex-wrap:wrap;border-top:1px solid #eceff1;\">\n<div style=\"flex:0 0 118px;padding:11px 14px;background:#F7FAFB;font-size:10.5px;letter-spacing:.09em;text-transform:uppercase;color:#6b8091;font-weight:600;line-height:1.5;\">Standartlar<\/div>\n<div style=\"flex:1 1 230px;min-width:0;padding:11px 14px;font-size:14.5px;line-height:1.7;color:#3d5260;word-wrap:break-word;overflow-wrap:break-word;\">AMS NUMARASI YOKTUR (bkz. standart notu). ASTM\/ASME: ASTM B333 \/ ASME SB-333 (levha, sac, \u015ferit) \u00b7 ASTM B335 \/ SB-335 (k\u00fct\u00fck, \u00e7ubuk) \u00b7 ASTM B622 \/ SB-622 (diki\u015fsiz boru ve t\u00fcp) \u00b7 ASTM B619 \/ SB-619 (diki\u015fli boru) \u00b7 ASTM B626 \/ SB-626 (diki\u015fli t\u00fcp) \u00b7 ASTM B564 \/ SB-564 (d\u00f6vme) \u00b7 ASTM B462 \/ SB-462 (d\u00f6vme veya haddelenmi\u015f flan\u015f, fitting, valf par\u00e7as\u0131) \u00b7 ASTM B366 \/ SB-366 (fabrikada \u00fcretilmi\u015f d\u00f6vme fitting; s\u0131n\u0131f i\u015fareti CRHB3). Avrupa: DIN 17744 (2.4600 NiMo29Cr) \u00b7 DIN 17750\/17751\/17752\/17754 \u00b7 VdT\u00dcV Werkstoffblatt 517. Kaynak sarf malzemesi: AWS A5.14 \/ SFA-5.14 ERNiMo-10 (\u00e7\u0131plak tel) \u00b7 AWS A5.11 \/ SFA-5.11 ENiMo-10 (\u00f6rt\u00fcl\u00fc elektrot) \u00b7 DIN 2.4695 (tel) \u00b7 DIN 2.4696 (elektrot). Kod: ASME BPVC B\u00f6l\u00fcm VIII Div. 1 ve ASME B31.3 i\u00e7in tavan 427 \u00b0C (800 \u00b0F) \u00b7 ASME B\u00f6l\u00fcm XII i\u00e7in 343 \u00b0C (650 \u00b0F) \u00b7 ASME Code Case 2140 \u00b7 ASME B\u00f6l\u00fcm IX P-No. 44, F-No. 44.<br \/><span style=\"font-size:12.5px;color:#7b8f9b;line-height:1.6;display:inline-block;margin-top:6px;\">N10675 \u0130\u00c7\u0130N DO\u011eRULANMI\u015e B\u0130R AMS \u015eARTNAMES\u0130 BULUNAMAMI\u015eTIR. Piyasada B-3 ile birlikte an\u0131lan iki numara TEK TEK kontrol edilmi\u015f ve \u0130K\u0130S\u0130 DE BA\u015eKA ALA\u015eIMA \u00c7IKMI\u015eTIR: (1) AMS 5891 \u2014 SAE&#8217;nin kendi kay\u0131t ba\u015fl\u0131\u011f\u0131 &#8216;Nickel Alloy, Corrosion and Heat-Resistant, Bars,\u2026<\/span><\/div>\n<\/div>\n<div style=\"display:flex;flex-wrap:wrap;border-top:1px solid #eceff1;\">\n<div style=\"flex:0 0 118px;padding:11px 14px;background:#F7FAFB;font-size:10.5px;letter-spacing:.09em;text-transform:uppercase;color:#6b8091;font-weight:600;line-height:1.5;\">Art\u0131s\u0131<\/div>\n<div style=\"flex:1 1 230px;min-width:0;padding:11px 14px;font-size:14.5px;line-height:1.7;color:#3d5260;word-wrap:break-word;overflow-wrap:break-word;\">Her deri\u015fim ve her s\u0131cakl\u0131kta hidroklorik asit direnci: %20 HCl&#8217;de bildirilen korozyon h\u0131z\u0131 0,305 mm\/y\u0131l (Virgamet), tipik HCl servis de\u011ferleri 0,13 mm\/y\u0131l alt\u0131nda bildirilmi\u015ftir.<\/div>\n<\/div>\n<div style=\"display:flex;flex-wrap:wrap;border-top:1px solid #eceff1;\">\n<div style=\"flex:0 0 118px;padding:11px 14px;background:#F7FAFB;font-size:10.5px;letter-spacing:.09em;text-transform:uppercase;color:#6b8091;font-weight:600;line-height:1.5;\">Kaynak<\/div>\n<div style=\"flex:1 1 230px;min-width:0;padding:11px 14px;font-size:14.5px;line-height:1.7;color:#3d5260;word-wrap:break-word;overflow-wrap:break-word;\">GTAW\/TIG, GMAW\/MIG ve SMAW\/\u00f6rt\u00fcl\u00fc elektrot ile kaynak edilir. Dolgu metali: ERNiMo-10 (\u00e7\u0131plak tel, AWS A5.14) ve ENiMo-10 (\u00f6rt\u00fcl\u00fc elektrot, AWS A5.11); Avrupa taraf\u0131nda SG-NiMo30Cr. \u00d6N TAV GEREKMEZ.<\/div>\n<\/div>\n<div style=\"display:flex;flex-wrap:wrap;border-top:1px solid #eceff1;\">\n<div style=\"flex:0 0 118px;padding:11px 14px;background:#fdeceb;font-size:10.5px;letter-spacing:.09em;text-transform:uppercase;color:#c0392b;font-weight:600;line-height:1.5;\">S\u0131n\u0131rlar\u0131<\/div>\n<div style=\"flex:1 1 230px;min-width:0;padding:11px 14px;font-size:14.5px;line-height:1.7;color:#3d5260;word-wrap:break-word;overflow-wrap:break-word;background:#fdeceb;\">1) Y\u00dcKSELTGEY\u0130C\u0130 ORTAMDA KULLANILMAZ \u2014 bu ala\u015f\u0131m\u0131n tek ve en sert s\u0131n\u0131r\u0131 budur. Ala\u015f\u0131mda krom yaln\u0131zca %1-3&#8217;t\u00fcr; y\u00fckseltgeyici ortam\u0131 ta\u015f\u0131yacak krom yoktur.<\/div>\n<\/div>\n<div style=\"padding:14px;border-top:1px solid #eceff1;\"><a href=\"https:\/\/www.defencemetal.com\/index.php\/bize-ulasin\/\" style=\"display:inline-block;padding:11px 20px;font-size:14px;font-weight:700;text-decoration:none;margin:0 8px 6px 0;background:#dd3333;color:#ffffff;\">TEKL\u0130F \u0130STE<\/a><a href=\"https:\/\/www.defencemetal.com\/index.php\/nikel-alasimlari-inconel-monel-invar-defence-metal\/\" style=\"display:inline-block;padding:11px 20px;font-size:14px;font-weight:700;text-decoration:none;margin:0 8px 6px 0;font-weight:600;border:1px solid #12303f;color:#12303f;\">T\u00fcm nikel ala\u015f\u0131mlar\u0131 &rarr;<\/a><span data-dm=\"dm-teknik\" style=\"cursor:pointer;display:inline-block;padding:11px 20px;font-size:14px;font-weight:700;text-decoration:none;margin:0 8px 6px 0;border:1px solid #dd3333;color:#dd3333;\">TEKN\u0130K DETAYLAR &darr;<\/span><\/div>\n<div style=\"padding:9px 14px;border-top:1px solid #eceff1;font-size:11.5px;color:#8a9aa4;line-height:1.5;\">Veriler \u00fcretici veri sayfalar\u0131ndan derlenmi\u015ftir &middot; sipari\u015f \u00f6ncesi g\u00fcncel \u015fartnameden teyit ediniz<\/div>\n<\/div>\n<\/div>\n<p><!-- \/dm-hap --><!-- dm-nav --><\/p>\n<style>h4[id^=\"dm-b\"]{scroll-margin-top:120px}#dm-teknik{scroll-margin-top:120px}<\/style>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:0 0 22px;padding:12px 14px;\">\n<div style=\"font-size:10.5px;letter-spacing:.09em;text-transform:uppercase;color:#6b8091;font-weight:600;margin-bottom:9px;\">Bu sayfada &middot; t\u0131klay\u0131n, ilgili b\u00f6l\u00fcme gider<\/div>\n<div><span data-dm=\"dm-b0\" style=\"cursor:pointer;display:inline-block;padding:5px 11px;border:1px solid #dfe6ea;background:#F7FAFB;margin:0 6px 7px 0;font-size:13px;color:#12303f;\">Hastelloy B-3 Nedir<\/span><span data-dm=\"dm-b1\" style=\"cursor:pointer;display:inline-block;padding:5px 11px;border:1px solid #dfe6ea;background:#F7FAFB;margin:0 6px 7px 0;font-size:13px;color:#12303f;\">\u00dcr\u00fcn Formuna G\u00f6re Standartlar<\/span><span data-dm=\"dm-b2\" style=\"cursor:pointer;display:inline-block;padding:5px 11px;border:1px solid #dfe6ea;background:#F7FAFB;margin:0 6px 7px 0;font-size:13px;color:#12303f;\">Standard\u0131 OLMAYAN \u00dcr\u00fcn Formlar\u0131<\/span><span data-dm=\"dm-b3\" style=\"cursor:pointer;display:inline-block;padding:5px 11px;border:1px solid #dfe6ea;background:#F7FAFB;margin:0 6px 7px 0;font-size:13px;color:#12303f;\">Kimyasal Bile\u015fim<\/span><span data-dm=\"dm-b4\" style=\"cursor:pointer;display:inline-block;padding:5px 11px;border:1px solid #dfe6ea;background:#F7FAFB;margin:0 6px 7px 0;font-size:13px;color:#12303f;\">Mekanik De\u011ferler<\/span><span data-dm=\"dm-b5\" style=\"cursor:pointer;display:inline-block;padding:5px 11px;border:1px solid #dfe6ea;background:#F7FAFB;margin:0 6px 7px 0;font-size:13px;color:#12303f;\">Fiziksel \u00d6zellikler<\/span><span data-dm=\"dm-b6\" style=\"cursor:pointer;display:inline-block;padding:5px 11px;border:1px solid #dfe6ea;background:#F7FAFB;margin:0 6px 7px 0;font-size:13px;color:#12303f;\">Is\u0131l \u0130\u015flem ve Is\u0131l Kararl\u0131l\u0131k<\/span><span data-dm=\"dm-b7\" style=\"cursor:pointer;display:inline-block;padding:5px 11px;border:1px solid #dfe6ea;background:#F7FAFB;margin:0 6px 7px 0;font-size:13px;color:#12303f;\">Kaynak<\/span><span data-dm=\"dm-b8\" style=\"cursor:pointer;display:inline-block;padding:5px 11px;border:1px solid #dfe6ea;background:#F7FAFB;margin:0 6px 7px 0;font-size:13px;color:#12303f;\">Tala\u015fl\u0131 \u0130malat<\/span><span data-dm=\"dm-b9\" style=\"cursor:pointer;display:inline-block;padding:5px 11px;border:1px solid #dfe6ea;background:#F7FAFB;margin:0 6px 7px 0;font-size:13px;color:#12303f;\">Korozyon<\/span><span data-dm=\"dm-b10\" style=\"cursor:pointer;display:inline-block;padding:5px 11px;border:1px solid #dfe6ea;background:#F7FAFB;margin:0 6px 7px 0;font-size:13px;color:#12303f;\">S\u0131k Sorulan Sorular<\/span><\/div>\n<\/div>\n<p><script>(function(){function go(id){var e=document.getElementById(id);if(e){var s=document.scrollingElement||document.documentElement;var y=e.getBoundingClientRect().top+s.scrollTop-118;if(y-0-0-0-0!==y){y=0;}window.scrollTo(0,y);}}function bind(el){el.addEventListener(\"click\",function(ev){ev.preventDefault();go(el.getAttribute(\"data-dm\"));});}function init(){var l=document.querySelectorAll(\"[data-dm]\");Array.prototype.forEach.call(l,bind);if(location.hash){if(location.hash.indexOf(\"#dm-\")===0){try{history.replaceState(null,\"\",location.pathname+location.search);}catch(e){}window.scrollTo(0,0);setTimeout(function(){window.scrollTo(0,0);},80);}}}if(document.readyState===\"loading\"){document.addEventListener(\"DOMContentLoaded\",init);}else{init();}})();<\/script><!-- \/dm-nav --><br \/>\n<span id=\"dm-teknik\" style=\"display:block;height:0;overflow:hidden;\"><\/span><br \/>\nHastelloy B-3 (UNS N10675) veya di\u011fer yayg\u0131n olarak kullan\u0131lan ad\u0131yla Alloy B-3 malzeme <a href=\"https:\/\/www.defencemetal.com\/index.php\/nikel-alasimlari-inconel-monel-invar-defence-metal\/\">nikel ala\u015f\u0131m malzemeler<\/a> aras\u0131nda Hastelloy malzemeler grubuna giren olduk\u00e7a \u00f6zel bir malzemedir. Hastelloy malzemeler aras\u0131nda kullan\u0131m\u0131 \u00e7ok yayg\u0131n olmayan bu kalite malzeme, \u00f6zellikle saf hidroklorik asit olan yerlerde, <a href=\"https:\/\/en.wikipedia.org\/wiki\/Hydrobromic_acid\">hidrobomik asit<\/a> olan yerlerde ve s\u00fclfirik asit olan yerlerde bu tarz asitlere uzun s\u00fcre dayanabildi\u011fi i\u00e7in tercih edilen bir malzemedir.<\/p>\n<p>Bu malzeme\u00a0yakla\u015f\u0131k %65 nikel elementi, yakla\u015f\u0131k % 29 molibden elementi, ~% 3 tungsten ve cobalt gibi olduk\u00e7a zor ko\u015fullara dayan\u0131m\u0131 artt\u0131ran elementler i\u00e7ermektedir. T\u00fcm bu i\u00e7erdi\u011fi elementler bu kalite malzemenin \u00fcretimini zorla\u015ft\u0131rmaktad\u0131r. Ayr\u0131ca t\u00fcm bu elementler pahal\u0131 elemenler oldu\u011fu i\u00e7in bu malzemeler oluk\u00e7a pahal\u0131 malzemelerdir.<\/p>\n<p><strong>\u0130\u015flenebilirlik: <\/strong>Hastelloy B-3, y\u00fcksek nikel i\u00e7eri\u011fi ve molibden katk\u0131lar\u0131 ile y\u00fcksek mukavemet g\u00f6steren bir ala\u015f\u0131md\u0131r. Bu, i\u015flenebilirlik a\u00e7\u0131s\u0131ndan baz\u0131 zorluklar olu\u015fturabilir, ancak dikkatli i\u015fleme y\u00f6ntemleriyle verimli sonu\u00e7lar al\u0131nabilir.<\/p>\n<p><strong>Tornalama ve Frezeleme<\/strong>:<\/p>\n<ul>\n<li><strong>Kesici Tak\u0131mlar<\/strong>: Genellikle sertle\u015ftirilmi\u015f \u00e7elik ve karb\u00fcr u\u00e7lar kullan\u0131l\u0131r. Bu t\u00fcr u\u00e7lar, y\u00fcksek sertlik ve s\u0131cakl\u0131k dayan\u0131m\u0131na kar\u015f\u0131 diren\u00e7 sa\u011flar.<\/li>\n<li><strong>Kesme H\u0131z\u0131<\/strong>: D\u00fc\u015f\u00fck ve orta kesme h\u0131zlar\u0131 genellikle daha iyi sonu\u00e7lar verir. A\u015f\u0131r\u0131 y\u00fcksek h\u0131zlar a\u015f\u0131nmay\u0131 h\u0131zland\u0131rabilir ve i\u015fleme kalitesini d\u00fc\u015f\u00fcrebilir.<\/li>\n<li><strong>So\u011futma<\/strong>: So\u011futma s\u0131v\u0131lar\u0131 kullanmak, a\u015f\u0131r\u0131 \u0131s\u0131nmay\u0131 \u00f6nlemeye yard\u0131mc\u0131 olur ve i\u015fleme kalitesini art\u0131r\u0131r. So\u011futma s\u0131v\u0131lar\u0131n\u0131n kimyasal reaksiyonlara neden olmayacak t\u00fcrde olmas\u0131 \u00f6nemlidir.<\/li>\n<\/ul>\n<p><strong>Kaynaklanabilirlik<\/strong>: TIG ve MIG kaynak i\u015flemleriyle kaynaklanabilir. Kaynak s\u0131ras\u0131nda dikkat edilmesi gereken en \u00f6nemli fakt\u00f6r, y\u00fcksek \u0131s\u0131l gerilim ve oksitlenme riski oldu\u011fundan, kaynak \u00f6ncesi ve sonras\u0131 temizlik \u00f6nemlidir. Y\u00fcksek \u0131s\u0131l gerilim kaynak s\u0131ras\u0131nda ala\u015f\u0131m\u0131n korozyon direncini azaltabilir, bu nedenle kaynak i\u015flemi s\u0131ras\u0131nda koruyucu gazlar kullan\u0131lmas\u0131 ve i\u015flem s\u0131cakl\u0131klar\u0131n\u0131n kontrol edilmesi \u00f6nerilir.<\/p>\n<p><strong>Is\u0131l \u0130\u015flem<\/strong>: Genellikle \u0131s\u0131l i\u015fleme tabi tutulmaz \u00e7\u00fcnk\u00fc ala\u015f\u0131m zaten y\u00fcksek s\u0131cakl\u0131k dayan\u0131m\u0131na sahiptir. Bunun yerine, kaynak ve \u015fekillendirme i\u015flemleri s\u0131ras\u0131nda malzemenin s\u0131cakl\u0131k toleranslar\u0131na dikkat edilmelidir.<\/p>\n<div data-dmtp=\"1\" style=\"position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span>\n<table id=\"tablepress-45\" class=\"tablepress tablepress-id-45\">\n<thead>\n<tr class=\"row-1\">\n\t<th class=\"column-1\">Kimyasal Bile\u015fimi (NiMo29Cr)<br \/>\n<strong><\/th><td class=\"column-2\"><\/td><th class=\"column-3\">Oda S\u0131cakl\u0131\u011f\u0131ndaki Mekanik \u00d6zellikleri<br \/>\n<strong><\/th><td class=\"column-4\"><\/td><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<tr class=\"row-2\">\n\t<th class=\"column-1\">Kalite <strong><\/th><th class=\"column-2\">Hastelloy B-3 (UNS N10675)<\/th><th class=\"column-3\">\u00d6zellikler<\/th><th class=\"column-4\">De\u011ferler<\/th><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<\/thead>\n<tbody class=\"row-hover\">\n<tr class=\"row-3\">\n\t<td class=\"column-1\">Ni<\/td><td class=\"column-2\">min %65<\/td><td class=\"column-3\">\u00d6z k\u00fctlesi (\u00d6zg\u00fcl a\u011f\u0131rl\u0131\u011f\u0131)<\/td><td class=\"column-4\">9220 kg\/m\u00b3<\/td><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<tr class=\"row-4\">\n\t<td class=\"column-1\">Cr<\/td><td class=\"column-2\">max %1.5<\/td><td class=\"column-3\">Erime S\u0131cakl\u0131\u011f\u0131<\/td><td class=\"column-4\">1370 \u2013 1420 \u00b0C aras\u0131<\/td><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<tr class=\"row-5\">\n\t<td class=\"column-1\">Fe<\/td><td class=\"column-2\">max %1.5<\/td><td class=\"column-3\"><\/td><td class=\"column-4\"><\/td><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<tr class=\"row-6\">\n\t<td class=\"column-1\">Mo<\/td><td class=\"column-2\">~%28.5<\/td><td class=\"column-3\"><\/td><td class=\"column-4\"><\/td><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<tr class=\"row-7\">\n\t<td class=\"column-1\">Tungsten<\/td><td class=\"column-2\">max %3<\/td><td class=\"column-3\"><\/td><td class=\"column-4\"><\/td><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<tr class=\"row-8\">\n\t<td class=\"column-1\">C<\/td><td class=\"column-2\">max %0.01<\/td><td class=\"column-3\"><\/td><td class=\"column-4\"><\/td><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<tr class=\"row-9\">\n\t<td class=\"column-1\">Mn<\/td><td class=\"column-2\">max %3<\/td><td class=\"column-3\"><\/td><td class=\"column-4\"><\/td><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<tr class=\"row-10\">\n\t<td class=\"column-1\">Si<\/td><td class=\"column-2\">max %0.1<\/td><td class=\"column-3\"><\/td><td class=\"column-4\"><\/td><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<tr class=\"row-11\">\n\t<td class=\"column-1\">Al<\/td><td class=\"column-2\">max %0.5<\/td><td class=\"column-3\"><\/td><td class=\"column-4\"><\/td><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<tr class=\"row-12\">\n\t<td class=\"column-1\">Co<\/td><td class=\"column-2\">max %3<\/td><td class=\"column-3\"><\/td><td class=\"column-4\"><\/td><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<tr class=\"row-13\">\n\t<td class=\"column-1\">Ti<\/td><td class=\"column-2\">max %0.2<\/td><td class=\"column-3\"><\/td><td class=\"column-4\"><\/td><td class=\"column-5\"><\/td><td class=\"column-6\"><\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p><!-- dm-benzer --><\/p>\n<div class=\"dm-benzer\" style=\"margin:22px 0 0;padding:14px 16px;border:1px solid #e0e0e0;background:#FBFCFD;\">\n<p style=\"font-size:11px;font-weight:700;letter-spacing:.08em;text-transform:uppercase;color:#9aa3a8;margin:0 0 8px;line-height:1.4;\">Benzer \u00fcr\u00fcnler<\/p>\n<p style=\"margin:0;font-size:15px;line-height:2;color:#333;\"><a href=\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-c-22\/\" style=\"color:#24BEE5;font-weight:600;text-decoration:none;\">Hastelloy C-22<\/a> &nbsp;\u00b7&nbsp; <a href=\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-c-276\/\" style=\"color:#24BEE5;font-weight:600;text-decoration:none;\">Hastelloy C-276<\/a> &nbsp;\u00b7&nbsp; <a href=\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-c-2000\/\" style=\"color:#24BEE5;font-weight:600;text-decoration:none;\">Hastelloy C-2000<\/a> &nbsp;\u00b7&nbsp; <a href=\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-x\/\" style=\"color:#24BEE5;font-weight:600;text-decoration:none;\">Hastelloy X<\/a> &nbsp;\u00b7&nbsp; <a href=\"https:\/\/www.defencemetal.com\/index.php\/nikel-alasimlari-inconel-monel-invar-defence-metal\/\" style=\"color:#666;font-weight:600;text-decoration:none;\">T\u00fcm nikel ala\u015f\u0131mlar &rarr;<\/a><\/p>\n<\/div>\n<p><!-- \/dm-benzer --><\/p>\n<p><!-- dm-std --><\/p>\n<div class=\"dm-std\" style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">Standartlar ve Kar\u015f\u0131l\u0131klar\u0131 \u00b7 Hastelloy B-3<\/div>\n<div data-dmtw=\"1\" style=\"position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"position:relative;z-index:2;overflow-x:auto;\">\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Ticari ad<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">Hastelloy B-3<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">UNS<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">N10675<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">W.Nr (DIN\/EN)<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">2.4600<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">EN kimyasal sembol<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">NiMo29Cr<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">ASTM<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">B335 <span style=\"font-size:13px;color:#6b7a84;\">(\u00e7ubuk)<\/span> \u00b7 B564 <span style=\"font-size:13px;color:#6b7a84;\">(d\u00f6vme)<\/span> \u00b7 B333 <span style=\"font-size:13px;color:#6b7a84;\">(levha, sac)<\/span><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Temin edilebilen formlar<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">Yuvarlak \u00e7ubuk \u00b7 Lama \u00b7 Levha \u00b7 Sac \u00b7 Boru \u00b7 D\u00f6vme<br \/><span style=\"font-size:13px;color:#6b7a84;\">T\u00fcm formlar sipari\u015f bazl\u0131 temin edilmektedir.<\/span><\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<\/div>\n<\/div>\n<p><!-- \/dm-std --><\/p>\n<p><!-- dm-zengin --><\/p>\n<h4 id=\"dm-b0\" style=\"font-size:19px;font-weight:700;color:#12303f;margin:30px 0 10px;line-height:1.35;\">Hastelloy B-3 Nedir \u2014 ve B, B-2, B-3 Aras\u0131ndaki Ger\u00e7ek Fark<\/h4>\n<p><!-- dm-diy-kars --><\/p>\n<div style=\"border:1px solid #e3e9ec;margin:22px 0 26px;background:#fff;position:relative;overflow:hidden;\">\n<div style=\"background:#12303f;color:#fff;padding:9px 14px;font-size:14px;font-weight:700;letter-spacing:.3px;position:relative;z-index:2;\">KAR\u015eILA\u015eTIRMA<\/div>\n<div style=\"position:relative;z-index:2;\">\n<div style=\"padding:10px 14px 0;font-size:12.5px;color:#5b7180;line-height:1.7;\">Is\u0131l kararl\u0131l\u0131k (ara faz \u00e7\u00f6kelmesi ve kaynak ITAB davran\u0131\u015f\u0131) \u00b7 \u015fartname minimumlar\u0131 \u00b7 ortam s\u0131n\u0131f\u0131 (indirgeyici \/ y\u00fckseltgeyici)<\/div>\n<div style=\"padding:8px 12px 0;font-size:13.5px;font-weight:700;color:#12303f;\">A \u00b7 ISIL KARARLILIK \u2014 B-3&#8217;\u00fcn varl\u0131k sebebi (Haynes International)<\/div>\n<div style=\"padding:12px 12px 2px;position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"overflow-x:auto;position:relative;z-index:2;\">\n<table style=\"width:100%;border-collapse:collapse;font-size:13.5px;min-width:430px;background:transparent;\">\n<tr>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">\u00d6l\u00e7\u00fct<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">B3<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">B2<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">Fark<\/th>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">Bask\u0131n zararl\u0131 faz<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Ni3Mo \u2014 YAVA\u015e olu\u015fur<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Ni4Mo \u2014 HIZLI olu\u015fur<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">B-3&#8217;te k\u00fc\u00e7\u00fck ala\u015f\u0131m ilaveleri ve ayarlanm\u0131\u015f molibden ile yava\u015f olu\u015fan Ni3Mo tercih edilmi\u015ftir.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">Gevrekle\u015fmenin h\u0131z\u0131<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">650 \u00b0C dolay\u0131nda zararl\u0131 faz\u0131n geli\u015fmesi SAATLER al\u0131r<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">750 \u00b0C dolay\u0131nda HIZLA Ni4Mo olu\u015fur<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">B-3&#8217;\u00fcn \u00f6l\u00e7\u00fclebilir \u00fcst\u00fcnl\u00fc\u011f\u00fc BURADADIR: \u015fekillendirme \u0131s\u0131tmalar\u0131nda ve kaynak ITAB&#8217;\u0131nda s\u00fcneklik korunur.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">Kaynak sonras\u0131 \u0131s\u0131l i\u015flem<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Kural olarak gerekmez (Zapp: \u00f6n tav veya sonradan \u0131s\u0131l i\u015flem genellikle gerekli de\u011fildir)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Ara faz \u00e7\u00f6kelmesi nedeniyle kaynak sonras\u0131 davran\u0131\u015f sorunludur<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">B-3 do\u011frudan bu sorunu \u00e7\u00f6zmek i\u00e7in geli\u015ftirilmi\u015ftir.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">Bile\u015fimdeki ayr\u0131m<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">Cr %1,0-3,0 ve Fe %1,0-3,0 KONTROLL\u00dc olarak vard\u0131r<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">Ni-Mo esasl\u0131d\u0131r; B-3&#8217;teki kontroll\u00fc Cr-Fe ayar\u0131 yoktur<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">Cr ve Fe burada korozyon i\u00e7in de\u011fil, FAZ KARARLILI\u011eI i\u00e7in eklenmi\u015ftir; %1-3 krom y\u00fckseltgeyici ortam direnci vermez.<\/td>\n<\/tr>\n<\/table>\n<\/div>\n<\/div>\n<div style=\"padding:8px 12px 0;font-size:13.5px;font-weight:700;color:#12303f;\">B \u00b7 \u015eARTNAME M\u0130N\u0130MUMLARI \u2014 ASTM B333 ve B335 (ayn\u0131 tablolar)<\/div>\n<div style=\"padding:12px 12px 2px;position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"overflow-x:auto;position:relative;z-index:2;\">\n<table style=\"width:100%;border-collapse:collapse;font-size:13.5px;min-width:430px;background:transparent;\">\n<tr>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">\u00d6l\u00e7\u00fct<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">B3<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">B2<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">Fark<\/th>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">\u00c7ekme dayan\u0131m\u0131 minimum<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">760 MPa (110 ksi)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">760 MPa (110 ksi)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">FARK YOK. ASTM B335 kapsam\u0131ndaki N10665, N10675, N10629 ve N10624 ayn\u0131 minimum seti ta\u015f\u0131r.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">Akma dayan\u0131m\u0131 minimum<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">350 MPa (51 ksi)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">350 MPa (51 ksi)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">FARK YOK.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">Uzama minimum<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">%40<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">%40<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">FARK YOK. SONU\u00c7: B-3 B\u0130R MUKAVEMET Y\u00dcKSELTMES\u0130 DE\u011e\u0130LD\u0130R; kazan\u00e7 yaln\u0131zca \u0131s\u0131l kararl\u0131l\u0131ktad\u0131r.<\/td>\n<\/tr>\n<\/table>\n<\/div>\n<\/div>\n<div style=\"padding:8px 12px 0;font-size:13.5px;font-weight:700;color:#12303f;\">C \u00b7 ORTAM SINIFI \u2014 B ailesi ile C ailesi nerede ayr\u0131l\u0131r<\/div>\n<div style=\"padding:12px 12px 2px;position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"overflow-x:auto;position:relative;z-index:2;\">\n<table style=\"width:100%;border-collapse:collapse;font-size:13.5px;min-width:430px;background:transparent;\">\n<tr>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">\u00d6l\u00e7\u00fct<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">B3<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">C ailesi<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">Fark<\/th>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">Krom i\u00e7eri\u011fi<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">%1,0-3,0<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">C-276 %14,5-16,5 \u00b7 C-22 %20,0-22,5<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Krom y\u00fckseltgeyici ortam\u0131 ta\u015f\u0131r. B-3&#8217;te bu krom YOKTUR.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">\u0130ndirgeyici asit (HCl, H2SO4)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">\u00c7al\u0131\u015fma alan\u0131. Her deri\u015fim ve her s\u0131cakl\u0131kta HCl.<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">S\u0131n\u0131rl\u0131; C-2000 %10 HCl&#8217;e kadar \u00fcst\u00fcn bildirilmi\u015ftir.<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">B-3 lehine.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">Ferrik (Fe3+) ve kuprik (Cu2+) tuzlar<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">KULLANILMAZ \u2014 h\u0131zl\u0131 korozyon ar\u0131zas\u0131<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Bu ortamlar\u0131n ala\u015f\u0131m\u0131d\u0131r<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Bu sat\u0131r bir tercih de\u011fil, bir YASAKTIR.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">ASME kod s\u0131cakl\u0131k tavan\u0131<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">427 \u00b0C (B\u00f6l\u00fcm VIII Div. 1, B31.3)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">C-22 i\u00e7in 677 \u00b0C (B\u00f6l\u00fcm I ve B\u00f6l\u00fcm VIII Div. 1)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">C ailesi lehine; B-3 bir y\u00fcksek s\u0131cakl\u0131k ala\u015f\u0131m\u0131 de\u011fildir.<\/td>\n<\/tr>\n<\/table>\n<\/div>\n<\/div>\n<div style=\"padding:10px 12px 2px;position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"position:relative;z-index:2;\">\n<div style=\"font-size:13.5px;font-weight:700;color:#12303f;margin:6px 0 6px;\">Ek bilgiler<\/div>\n<table style=\"width:100%;border-collapse:collapse;font-size:13.5px;background:transparent;\">\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">Kar\u015f\u0131la\u015ft\u0131r\u0131lan<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Hastelloy B-3 (UNS N10675) \u2014 Hastelloy B-2 (UNS N10665) \u2014 ve C ailesi (C-276 \/ C-22) ile \u00e7al\u0131\u015fma alan\u0131 ayr\u0131m\u0131<\/td>\n<\/tr>\n<\/table>\n<\/div>\n<\/div>\n<\/div>\n<div style=\"padding:6px 14px 12px;font-size:12px;color:#5b7180;line-height:1.7;border-top:1px solid #f0f3f5;position:relative;z-index:2;\">KURAL: her blok TEK B\u0130R KAYNAK A\u0130LES\u0130N\u0130N i\u00e7inden okunur; bloklar birbiriyle toplanmaz ve ayn\u0131 eksene konmaz. A blo\u011fu Haynes International&#8217;\u0131n B-2\/B-3 \u0131s\u0131l kararl\u0131l\u0131k kar\u015f\u0131la\u015ft\u0131rmas\u0131ndan okunur. B blo\u011fu ASTM&#8217;nin kendi \u015fartname tablolar\u0131ndan (B333 ve B335, her iki UNS de bu \u015fartnamelerin kapsam\u0131ndad\u0131r, yani ayn\u0131 kabul \u00f6l\u00e7\u00fct\u00fc alt\u0131ndad\u0131r) okunur. C blo\u011fu ortam s\u0131n\u0131f\u0131 ayr\u0131m\u0131d\u0131r ve \u00fcretici metinlerinin ORTAK ifadesidir, say\u0131sal bir korozyon testi de\u011fildir. A blo\u011fu TEK KURULU\u015eTAN (Haynes International) okunmu\u015ftur; B-2 ile B-3&#8217;\u00fc ayn\u0131 metinde kar\u015f\u0131la\u015ft\u0131ran ba\u015fka bir ba\u011f\u0131ms\u0131z \u00fcretici metni bulunamam\u0131\u015ft\u0131r. Blok bu nedenle kaynak ad\u0131yla etiketlenmi\u015ftir. B blo\u011fundaki SONU\u00c7 \u00f6nemlidir ve pazarlama diline ayk\u0131r\u0131d\u0131r: B-3&#8217;\u00fcn B-2&#8217;ye g\u00f6re \u015eARTNAME M\u0130N\u0130MUMU \u00dcST\u00dcNL\u00dc\u011e\u00dc YOKTUR. Kazan\u00e7 yaln\u0131zca \u0131s\u0131l kararl\u0131l\u0131ktad\u0131r. C blo\u011fundaki C-276 ve C-22 krom-molibden de\u011ferleri bu projenin C-276 ve C-22 kartlar\u0131ndan, ayn\u0131 ASTM \u015fartname tablolar\u0131ndan al\u0131nm\u0131\u015ft\u0131r.<\/div>\n<\/div>\n<p><!-- \/dm-diy-kars --><\/p>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\">Hastelloy B-3 (UNS <b>N10675<\/b> \/ W.Nr. <b>2.4600<\/b> \/ DIN <b>NiMo29Cr<\/b>), tek fazl\u0131 YMK (\u03b3) <b>nikel-molibden kat\u0131 \u00e7\u00f6zelti<\/b> ala\u015f\u0131m\u0131d\u0131r: nominal <b>%65 Ni \u2013 %28,5 Mo<\/b>, bilin\u00e7li olarak k\u00fc\u00e7\u00fck tutulmu\u015f Cr ve Fe, ve fiilen karbonsuz (<b>C \u2264%0,010<\/b>). <b>Kayda de\u011fer krom i\u00e7ermez<\/b> (%1,0\u20133,0) \u2014 ve bu tek olgu, ala\u015f\u0131m\u0131n hem ola\u011fan\u00fcst\u00fc oldu\u011fu her \u015feyi hem de ba\u015far\u0131s\u0131z oldu\u011fu her \u015feyi a\u00e7\u0131klar. <b>Bu bir indirgeyici asit ala\u015f\u0131m\u0131d\u0131r, genel ama\u00e7l\u0131 bir korozyon ala\u015f\u0131m\u0131 de\u011fildir.<\/b><\/p>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>Al\u0131c\u0131lar\u0131n ve hatta baz\u0131 veri sayfalar\u0131n\u0131n birbirine kar\u0131\u015ft\u0131rd\u0131\u011f\u0131 iki bamba\u015fka hasar mekanizmas\u0131 vard\u0131r.<\/b> Ayn\u0131 sorun de\u011fildirler ve 30 y\u0131l arayla \u00e7\u00f6z\u00fclm\u00fc\u015flerdir.<\/p>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">\u00dc\u00e7 Ku\u015fak \u00b7 \u0130ki Ayr\u0131 Metalurjik Sorun<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Ala\u015f\u0131m B<\/b><br \/>(N10001 \/ 2.4800)<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>Sorun: karb\u00fcr \u00e7\u00f6kelmesi.<\/b> C \u2264%0,05, Fe %4,0\u20136,0, V %0,2\u20130,4. Zararl\u0131 \u00e7\u00f6kelti <b>M\u2086C karb\u00fcrleridir (Ni\u2083Mo\u2083C \/ Ni\u2082Mo\u2084C)<\/b>: kaynak s\u0131ras\u0131nda 1200 \u00b0C \u00fczerinde \u00e7\u00f6z\u00fcn\u00fcr, so\u011fuma s\u0131ras\u0131nda <b>tane s\u0131n\u0131rlar\u0131nda yeniden \u00e7\u00f6kelir<\/b>. Klasik <b>b\u0131\u00e7ak-\u00e7izgisi ata\u011f\u0131 (knife-line attack)<\/b>: ergime \u00e7izgisinin hemen yan\u0131ndaki dar bir bant duyarl\u0131la\u015f\u0131r ve ana metalden \u00e7ok daha h\u0131zl\u0131 taneler aras\u0131 korozyona u\u011frar. <b>Korozif servise girecek her par\u00e7a kaynak sonras\u0131 \u00e7\u00f6zelti tav\u0131 istiyordu<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Ala\u015f\u0131m B-2<\/b><br \/>(N10665 \/ 2.4617)<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>\u00c7\u00f6z\u00fcm: karbonu %0,02&#8217;ye indirmek<\/b>, Fe \u2264%2,0 ve Cr \u2264%1,0. <b>Karb\u00fcr sorunu \u00e7\u00f6z\u00fcld\u00fc.<\/b> Ama karbonun k\u0131smen maskeledi\u011fi <b>ikinci ve bamba\u015fka bir sorun<\/b> a\u00e7\u0131\u011fa \u00e7\u0131kt\u0131: <b>Ni-Mo kat\u0131 \u00e7\u00f6zeltisinin uzun menzilli d\u00fczenlenmesi<\/b> \u2014 <b>Ni\u2084Mo (\u03b2), Ni\u2083Mo ve Ni\u2082Mo<\/b> intermetalikleri. Bunlar &#8220;<b>\u00e7ok gevrektir ve tane s\u0131n\u0131rlar\u0131 boyunca \u00e7atlak ilerlemesini kolayla\u015ft\u0131r\u0131r<\/b>&#8221; ve &#8220;<b>B-2&#8217;de d\u00fczenlenme reaksiyonunun kineti\u011fi \u00e7ok h\u0131zl\u0131d\u0131r<\/b>&#8220;. \u00d6l\u00e7\u00fcm: <b>B-2, ~750 \u00b0C&#8217;de h\u0131zla Ni\u2084Mo olu\u015fturur<\/b> ve <b>700 \u00b0C&#8217;de 0,5\u20131,0 saatte 10+ Rockwell A puan\u0131 sertle\u015fir<\/b>. <b>Bu duyarl\u0131la\u015fma de\u011fil, D\u00dcZENLENME GEVREKLE\u015eMES\u0130D\u0130R<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Ala\u015f\u0131m B-3<\/b><br \/>(N10675 \/ 2.4600)<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>\u00c7\u00f6z\u00fcm, molibdeni \u00e7\u0131karmak de\u011fil, yerine koyucu ala\u015f\u0131m elementlerini B\u0130L\u0130N\u00c7L\u0130 OLARAK GER\u0130 EKLEMEKT\u0130<\/b> (ABD patenti 6.503.345). Tasar\u0131m kural\u0131: toplam yer alan ala\u015f\u0131m elementi (SAE) <b>at. %2,5\u20137,5<\/b>; <b>&#8220;SAE art\u0131 0,7 \u00d7 molibden, yakla\u015f\u0131k 18 ile 20 aras\u0131nda&#8221;<\/b>; Ni at. %73\u201377, Mo at. %18\u201323<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">B-3&#8217;te Hangi \u0130lave Ne Yap\u0131yor (patentin kendi ifadeleriyle)<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Krom (%1,0\u20133,0)<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>Anahtar kararl\u0131la\u015ft\u0131r\u0131c\u0131.<\/b> &#8220;Bu ala\u015f\u0131mlarda daha kararl\u0131 bir <b>Ni\u2082(Mo,Cr)<\/b> faz\u0131 olu\u015fturuyor gibi g\u00f6r\u00fcn\u00fcyor&#8221; \u2014 yani reaksiyonu gevrek Ni\u2084Mo&#8217;dan <b>sapt\u0131r\u0131r<\/b>. <b>~%4 Cr \u00fczerinde uzama bozuluyor ve korozyon h\u0131zlar\u0131 y\u00fckseliyordu<\/b> \u2014 %3 tavan\u0131n\u0131n sebebi budur<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Demir (%1,0\u20133,0)<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">D\u00fczenlenmeyi bozar; ama korozyon h\u0131z\u0131n\u0131 orant\u0131l\u0131 olarak y\u00fckseltir. Patentin tercih etti\u011fi bant %1,5\u20133,5<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Manganez (\u2264%3,0)<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">&#8220;S\u0131cak i\u015flenebilirli\u011fi <b>ve metalurjik kararl\u0131l\u0131\u011f\u0131<\/b> iyile\u015ftirir&#8221;<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Al\u00fcminyum (\u2264%0,50)<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">Ergitmede deoksidan. Patentin tercih etti\u011fi %0,25\u20130,75<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Molibden kaymas\u0131<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">Nominal ~%28,5&#8217;e \u00e7\u0131kar\u0131ld\u0131 ve Ni\/Mo atom oran\u0131 <b>en k\u00f6t\u00fc d\u00fczenlenme penceresinin d\u0131\u015f\u0131na<\/b> ayarland\u0131<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p style=\"margin:18px 0 6px;font-size:15px;font-weight:700;color:#12303f;line-height:1.5;\">\u00d6l\u00e7\u00fclen sonu\u00e7 \u2014 \u00fcr\u00fcn sayfas\u0131na yaz\u0131lacak say\u0131lar<\/p>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>B-2:<\/b> ~750 \u00b0C&#8217;de h\u0131zla Ni\u2084Mo. <b>B-3:<\/b> &#8220;<b>~650 \u00b0C civar\u0131nda zararl\u0131 ikincil fazlar\u0131 olu\u015fturmak birka\u00e7 saat al\u0131r<\/b>&#8221; ve olu\u015fan faz Ni\u2084Mo de\u011fil, <b>daha yava\u015f olu\u015fan Ni\u2083Mo<\/b>&#8216;dur. Patent sertlik verisi: at. %5\u20135,5 SAE&#8217;li deneysel ala\u015f\u0131mlar &#8220;<b>700 \u00b0C&#8217;de 24 saat sonra bile kayda de\u011fer \u015fekilde sertle\u015fmedi<\/b>&#8221; \u2014 B-2&#8217;nin 0,5\u20131,0 saatte 10+ HRA&#8217;s\u0131na kar\u015f\u0131. <b>Ticari olarak belirleyici c\u00fcmle patentten geliyor:<\/b> &#8220;\u0131s\u0131tma veya so\u011futma s\u00fcreleri <b>B-2 ala\u015f\u0131m\u0131 i\u00e7in \u00f6nerilenlerden yakla\u015f\u0131k on kat daha yava\u015f<\/b> olabilir.&#8221; A\u011f\u0131r kesitleri kaynaklamay\u0131, yava\u015f so\u011futmay\u0131 ve ince kesitlerde havada so\u011futmay\u0131 m\u00fcmk\u00fcn k\u0131lan budur.<\/p>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>Korozyon sonucu<\/b> (\u00fcreticinin kendi kar\u015f\u0131la\u015ft\u0131rma testi): <b>700 \u00b0C&#8217;de maruziyetten sonra kaynar %60 H\u2082SO\u2084&#8217;te test \u2014 B-3: 24 saatte \u00e7atlama yok. B-2: 3 saatte taneler aras\u0131 \u00e7atlama.<\/b> <b>Uzun s\u00fcreli kararl\u0131l\u0131k:<\/b> <b>540 \u00b0C&#8217;de<\/b> maruziyetten sonra uzama <b>4.000 saatte %45,6; 8.000 saatte %47,1; 16.000 saatte %43,7<\/b> \u2014 iki y\u0131lda fiilen s\u00fcneklik kayb\u0131 yok.<\/p>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>Yay\u0131mlanmas\u0131 gereken uyar\u0131:<\/b> B-3 <b>daha yava\u015ft\u0131r, ba\u011f\u0131\u015f\u0131k de\u011fildir<\/b>. 650 \u00b0C&#8217;de birka\u00e7 saat h\u00e2l\u00e2 Ni\u2083Mo \u00fcretir. <b>B-3 bir y\u00fcksek s\u0131cakl\u0131k ala\u015f\u0131m\u0131 de\u011fildir ve 500\u2013900 \u00b0C band\u0131nda s\u00fcrekli servis i\u00e7in tasarlanmam\u0131\u015ft\u0131r.<\/b> Ayr\u0131ca iki iddiay\u0131 ayr\u0131 tutun: <b>b\u0131\u00e7ak-\u00e7izgisi ata\u011f\u0131na diren\u00e7 B-2&#8217;den devral\u0131nan d\u00fc\u015f\u00fck karbondan gelir; ITAB d\u00fczenlenme gevrekle\u015fmesine diren\u00e7 ise B-3&#8217;\u00fcn yeni katk\u0131s\u0131d\u0131r.<\/b><\/p>\n<h4 id=\"dm-b1\" style=\"font-size:19px;font-weight:700;color:#12303f;margin:30px 0 10px;line-height:1.35;\">\u00dcr\u00fcn Formuna G\u00f6re Standartlar<\/h4>\n<p><!-- dm-diy-std --><\/p>\n<div style=\"border:1px solid #e3e9ec;margin:22px 0 26px;background:#fff;position:relative;overflow:hidden;\">\n<div style=\"background:#12303f;color:#fff;padding:9px 14px;font-size:14px;font-weight:700;letter-spacing:.3px;position:relative;z-index:2;\">\u00dcR\u00dcN FORMUNA G\u00d6RE STANDARTLAR<\/div>\n<div style=\"position:relative;z-index:2;\">\n<div style=\"padding:12px 12px 2px;position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"overflow-x:auto;position:relative;z-index:2;\">\n<table style=\"width:100%;border-collapse:collapse;font-size:13.5px;min-width:430px;background:transparent;\">\n<tr>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">\u00dcr\u00fcn formu<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">Standartlar<\/th>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">Levha<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">ASTM B333 \/ ASME SB-333 \u2014 \u00e7\u00f6zelti tavl\u0131 ve tufalsiz \u00b7 DIN 17750 \u00b7 VdT\u00dcV Werkstoffblatt 517. AMS numaras\u0131 YOKTUR (bkz. standart notu).<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">Sac ve \u015ferit<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">ASTM B333 \/ ASME SB-333 \u2014 3\/16 in\u00e7 (4,76 mm) alt\u0131 sac ve \u015ferit ile 3\/16-2 1\/2 in\u00e7 levha AYNI minimum seti ta\u015f\u0131r \u00b7 DIN 17750. AMS numaras\u0131 YOKTUR.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">Yuvarlak \u00e7ubuk, lama ve k\u00fct\u00fck<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">ASTM B335 \/ ASME SB-335 \u2014 k\u00fct\u00fck, \u00e7ubuk ve bar; \u00e7\u00f6zelti tavl\u0131, asitlenmi\u015f veya mekanik olarak tufal\u0131 al\u0131nm\u0131\u015f \u00b7 DIN 17752. AMS numaras\u0131 YOKTUR.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">Diki\u015fsiz boru ve t\u00fcp<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">ASTM B622 \/ ASME SB-622 \u2014 \u00e7\u00f6zelti tavl\u0131 ve tufalsiz \u00b7 DIN 17751. AMS numaras\u0131 YOKTUR.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">Diki\u015fli boru (pipe)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">ASTM B619 \/ ASME SB-619 \u2014 S\u0131n\u0131f I: kaynakl\u0131 ve \u00e7\u00f6zelti tavl\u0131; S\u0131n\u0131f II: kaynakl\u0131, so\u011fuk i\u015flenmi\u015f ve \u00e7\u00f6zelti tavl\u0131. AMS numaras\u0131 YOKTUR.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">Diki\u015fli t\u00fcp<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">ASTM B626 \/ ASME SB-626. AMS numaras\u0131 YOKTUR.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">D\u00f6vme<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">ASTM B564 \/ ASME SB-564 \u2014 \u00e7\u00f6zelti tavl\u0131; N10675 bu \u015fartnamenin kapsam\u0131ndad\u0131r ve minimumlar\u0131 \u00e7ubukla ayn\u0131d\u0131r \u00b7 DIN 17754. AMS numaras\u0131 YOKTUR.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">Flan\u015f, valf par\u00e7as\u0131<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">ASTM B462 \/ ASME SB-462 \u2014 d\u00f6vme veya haddelenmi\u015f flan\u015f, fitting ve valf par\u00e7as\u0131; N10675 kapsamdad\u0131r \u00b7 boyut i\u00e7in ASME B16.5 \/ B16.47. AMS numaras\u0131 YOKTUR.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">Fitting (ba\u011flant\u0131 par\u00e7as\u0131)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">ASTM B366 \/ ASME SB-366 \u2014 fabrikada \u00fcretilmi\u015f d\u00f6vme fitting; N10675 kapsamdad\u0131r, s\u0131n\u0131f i\u015fareti CRHB3 \u00b7 boyut i\u00e7in ASME B16.9 \/ B16.11. AMS numaras\u0131 YOKTUR.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">Kaynak sarf malzemesi<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">AWS A5.14 \/ ASME SFA-5.14 ERNiMo-10 (\u00e7\u0131plak tel ve \u00e7ubuk) \u00b7 AWS A5.11 \/ ASME SFA-5.11 ENiMo-10 (\u00f6rt\u00fcl\u00fc elektrot) \u00b7 DIN 2.4695 (tel) \u00b7 DIN 2.4696 (elektrot) \u00b7 ASME B\u00f6l\u00fcm IX F-No. 44.<\/td>\n<\/tr>\n<\/table>\n<\/div>\n<\/div>\n<\/div>\n<div style=\"padding:6px 14px 12px;font-size:12px;color:#5b7180;line-height:1.7;border-top:1px solid #f0f3f5;position:relative;z-index:2;\">AMS numaralar\u0131 \u00f6nce yaz\u0131l\u0131r kural\u0131 bu ala\u015f\u0131mda uygulanamam\u0131\u015ft\u0131r: N10675 i\u00e7in do\u011frulanm\u0131\u015f AMS \u015fartnamesi YOKTUR. ASTM taraf\u0131nda dikkat \u00e7eken nokta: B333, B335, B564, B619, B622 ve B626 N10675 i\u00e7in AYNI minimum seti ta\u015f\u0131r \u2014 760 MPa \u00e7ekme, 350 MPa akma, %40 uzama. ASTM B462 ve B366 kapsam listelerinde N10675 do\u011frudan okunmu\u015ftur; B366&#8217;da s\u0131n\u0131f i\u015fareti CRHB3&#8217;t\u00fcr.<\/div>\n<\/div>\n<p><!-- \/dm-diy-std --><\/p>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">\u00dcr\u00fcn Formuna G\u00f6re Standartlar \u00b7 Hastelloy B-3 (N10675 \/ 2.4600)<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Levha \u00b7 sac \u00b7 \u015ferit<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">ASTM <b>B333<\/b> \/ ASME SB-333 \u2014 N10675 be\u015f kaliteden biridir (N10001, N10665, N10675, N10629, N10624)<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">\u00c7ubuk \u00b7 bar<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">ASTM <b>B335<\/b> \/ SB-335<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Yeniden d\u00f6vme i\u00e7in k\u00fct\u00fck\/bar<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">ASTM <b>B472<\/b> \u2014 <b>yaln\u0131zca \u00fcretici \u015fartname \u00e7izelgesinde<\/b>, ba\u011f\u0131ms\u0131z do\u011frulanamad\u0131<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Diki\u015fsiz boru ve t\u00fcp<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">ASTM <b>B622<\/b> \/ SB-622 \u2014 ASTM kapsam\u0131 t\u00fcp\u00fc <b>\u226488,9 mm (3\u00bd in\u00e7) D\u00c7<\/b> ile s\u0131n\u0131rlar<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Diki\u015fli boru<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">ASTM <b>B619<\/b> \/ SB-619<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Diki\u015fli t\u00fcp<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">ASTM <b>B626<\/b> \/ SB-626 \u2014 ASTM kapsam sayfas\u0131 <b>N10675&#8217;i a\u00e7\u0131k\u00e7a listeler<\/b>; \u215b\u20133\u00bd in\u00e7 D\u00c7, et 0,015\u20130,148 in\u00e7<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">D\u00f6vme ba\u011flant\u0131 par\u00e7alar\u0131<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">ASTM <b>B366<\/b> \/ SB-366 \u2014 standart do\u011fruland\u0131; <b>kalitenin kapsamda oldu\u011fu ba\u011f\u0131ms\u0131z do\u011frulanamad\u0131<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Flan\u015f \u00b7 d\u00f6vme fitting \u00b7 vana par\u00e7alar\u0131<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">ASTM <b>B462<\/b> \/ SB-462 \u2014 <b>ASTM ba\u015fl\u0131k\/kapsam\u0131 N10675&#8217;i ad\u0131yla sayar<\/b>; ba\u011flant\u0131 par\u00e7as\u0131 \u015fartnameleri i\u00e7inde en g\u00fc\u00e7l\u00fc do\u011frulama<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">D\u00f6vme<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">ASTM <b>B564<\/b> \/ SB-564 \u2014 kalite listesi ba\u011f\u0131ms\u0131z do\u011frulanamad\u0131<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">\u00c7\u0131plak kaynak teli<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>AWS A5.14 ERNiMo-10<\/b>, UNS <b>N10675<\/b> \u00b7 DIN kar\u015f\u0131l\u0131\u011f\u0131 <b>2.4695 \/ SG-NiMo30Cr<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">\u00d6rt\u00fcl\u00fc elektrot<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>AWS A5.11 ENiMo-10<\/b> \u00b7 DIN kar\u015f\u0131l\u0131\u011f\u0131 <b>2.4696 \/ EL-NiMo28Cr<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">ASME B\u00f6l\u00fcm IX<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">Ana metal <b>P-No. 44<\/b> \u00b7 Dolgu <b>F-No. 44<\/b> \u00b7 ISO\/TR 15608 Grup 44<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Avrupa<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">DIN 17744 <b>2.4600 NiMo29Cr<\/b> \u00b7 <b>VdT\u00dcV Malzeme Sayfas\u0131 517<\/b> \u00b7 sarf malzemeleri i\u00e7in VdT\u00dcV Kennblatt 7615\/7616\/7617<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Genel gereklilik belgesi<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>\u2014 do\u011frulanamad\u0131.<\/b> B333\/B335 kapsam sayfalar\u0131 bir refakat\u00e7i numara vermiyor. <b>Bir refakat\u00e7i numara yay\u0131mlamay\u0131n<\/b><\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">ASME Kod Kabul\u00fc ve AZAM\u0130 KOD SICAKLIKLARI (bunlar KOD limitleridir)<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>B\u00f6l\u00fcm VIII Div. 1<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>427 \u00b0C (800 \u00b0F)<\/b> \u2014 levha, sac, bar, d\u00f6vme, ba\u011flant\u0131 par\u00e7as\u0131, diki\u015fli ve diki\u015fsiz boru\/t\u00fcp<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>B\u00f6l\u00fcm VIII Div. 2<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>KABUL ED\u0130LM\u0130YOR<\/b> \u2014 Div. 2 tasar\u0131m\u0131nda B-3 kod davas\u0131 olmadan bas\u0131n\u00e7 s\u0131n\u0131r\u0131 malzemesi olamaz<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>B\u00f6l\u00fcm I (g\u00fc\u00e7 kazan\u0131)<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>KABUL ED\u0130LM\u0130YOR<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">B\u00f6l\u00fcm III S\u0131n\u0131f 2 \/ 3<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">427 \u00b0C<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">B\u00f6l\u00fcm XII (ta\u015f\u0131ma tank\u0131)<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>343 \u00b0C (650 \u00b0F)<\/b> \u2014 herkesin and\u0131\u011f\u0131 427 \u00b0C&#8217;nin epey alt\u0131nda<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">ASME B16.5 (flan\u015f) \u00b7 B16.34 (vana)<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">427 \u00b0C<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>ASME B31.1 (g\u00fc\u00e7 borulamas\u0131)<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>KABUL ED\u0130LM\u0130YOR<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">ASME B31.3 (proses borulamas\u0131)<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">427 \u00b0C<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>VdT\u00dcV 517<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>400 \u00b0C (752 \u00b0F)<\/b> \u2014 Avrupa yolunda tavan daha da d\u00fc\u015f\u00fckt\u00fcr<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">ASME Code Case 2140<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>Tek da\u011f\u0131t\u0131mc\u0131 iddias\u0131<\/b> \u2014 g\u00fcncel ASME code case listesinden teyit etmeden yay\u0131mlamay\u0131n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<h4 id=\"dm-b2\" style=\"font-size:19px;font-weight:700;color:#12303f;margin:30px 0 10px;line-height:1.35;\">Standard\u0131 OLMAYAN \u00dcr\u00fcn Formlar\u0131 \u2014 Ticari Olarak En De\u011ferli B\u00f6l\u00fcm<\/h4>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>Sat\u0131\u015f m\u00fchendislerinizin ezberlemesi gereken b\u00f6l\u00fcm budur.<\/b><\/p>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">N10675 i\u00e7in \u015eartname Bo\u015fluklar\u0131<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>So\u011fuk \u00e7ekilmi\u015f \/ yay teli<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>N10675 i\u00e7in ASTM (veya EN) tel \u00fcr\u00fcn \u015fartnamesi YOKTUR.<\/b> B472 <i>yeniden d\u00f6vme i\u00e7in k\u00fct\u00fck ve bar<\/i>d\u0131r; A5.14 bir <b>kaynak sarf malzemesi<\/b> \u015fartnamesidir ve yap\u0131sal tel \u015fartnamesi de\u011fildir. Tedarik\u00e7iler B-3 tel satar (tavl\u0131 &lt;1200 N\/mm\u00b2, yay temperi 1600\u20132000 N\/mm\u00b2, tek kaynakl\u0131) ama <b>firma \u015fartnamesine g\u00f6re<\/b> satarlar. &#8220;ASTM&#8217;ye g\u00f6re B-3 tel&#8221; talebinin d\u00fcr\u00fcst cevab\u0131: <b>kimya B335&#8217;e, mekanikler anla\u015fmaya g\u00f6re<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>D\u00f6k\u00fcm<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>B-3&#8217;\u00fcn d\u00f6k\u00fcm e\u015fde\u011feri YOKTUR.<\/b> D\u00f6k\u00fcm Ni-Mo kaliteleri ASTM A494 <b>N-12MV<\/b> ve <b>N-7M<\/b>&#8216;dir ve bunlar bile\u015fim olarak <b>ala\u015f\u0131m B \/ B-2<\/b>&#8216;ye kar\u015f\u0131l\u0131k gelir \u2014 N-12MV&#8217;nin y\u00fcksek demiri ve vanadyumu vard\u0131r. <b>Standartla\u015fm\u0131\u015f bir &#8220;B-3 d\u00f6k\u00fcm vana g\u00f6vdesi&#8221; diye bir \u00fcr\u00fcn yoktur.<\/b> D\u00f6vme sat\u0131n veya N-7M sat\u0131n ve <b>bunun B-3 olmad\u0131\u011f\u0131n\u0131 ve B-3&#8217;\u00fcn \u0131s\u0131l kararl\u0131l\u0131\u011f\u0131na sahip olmad\u0131\u011f\u0131n\u0131 a\u00e7\u0131k\u00e7a s\u00f6yleyin<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>C\u0131vata \u00b7 ba\u011flant\u0131 eleman\u0131<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>N10675 i\u00e7in adanm\u0131\u015f bir ASTM c\u0131vatalama \u015fartnamesi YOKTUR<\/b> (B637\/B473 tipi bir belge yok). B-3 ba\u011flant\u0131 elemanlar\u0131 <b>B335 \u00e7ubuktan al\u0131c\u0131n\u0131n resmine g\u00f6re<\/b> yap\u0131l\u0131r \u2014 teklifte bunu yaz\u0131n<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Havac\u0131l\u0131k (AMS)<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>B-3 i\u00e7in AMS \u015fartnamesi YOKTUR.<\/b> Da\u011f\u0131t\u0131mc\u0131 sayfalar\u0131nda dola\u015fan iki AMS numaras\u0131 da <b>ba\u015fka ala\u015f\u0131mlara aittir<\/b> (bkz. tuzaklar)<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>NACE MR0175 \/ ISO 15156<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>N10675&#8217;in ISO 15156-3 Ek A&#8217;da yer ald\u0131\u011f\u0131 DO\u011eRULANAMADI.<\/b> \u00dcreticinin kendi B-3 bro\u015f\u00fcr\u00fcnde ve ala\u015f\u0131m sayfas\u0131nda <b>hi\u00e7 NACE ifadesi yoktur<\/b> \u2014 oysa ayn\u0131 \u00fcretici C-276, C-22 ve 625 i\u00e7in NACE durumu yay\u0131mlar. ~%1,5 Cr ile ek\u015fi kuyulardaki y\u00fckseltgen ve elementel k\u00fck\u00fcrt ko\u015fullar\u0131nda ya\u015fayamaz. <b>Sayfaya \u015funu yaz\u0131n:<\/b> &#8220;B-3, NACE MR0175\/ISO 15156-3 kapsam\u0131nda listeli bir ek\u015fi servis malzemesi de\u011fildir. H\u2082S servisi i\u00e7in Ek A&#8217;ya do\u011frudan bak\u0131n; o g\u00f6rev i\u00e7in listeli nikel ala\u015f\u0131mlar\u0131 Ni-Cr-Mo kaliteleridir (N10276, N06022, N06625).&#8221; <b>Asla N10675 i\u00e7in &#8220;NACE MR0175 uyumlu&#8221; sertifika \u00e7\u0131karmay\u0131n<\/b><\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<h4 id=\"dm-b3\" style=\"font-size:19px;font-weight:700;color:#12303f;margin:30px 0 10px;line-height:1.35;\">Kimyasal Bile\u015fim<\/h4>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>ASTM B333 \/ B335 (ayn\u0131 tablo B619\/B622\/B626\/B462\/B564&#8217;e ta\u015f\u0131n\u0131r), a\u011f\u0131rl\u0131k\u00e7a %:<\/b> <b>Ni \u226565,0<\/b> \u00b7 <b>Mo 27,0\u201332,0<\/b> \u00b7 <b>Fe 1,0\u20133,0<\/b> \u00b7 <b>Cr 1,0\u20133,0<\/b> \u00b7 <b>Ni + Mo 94,0\u201398,0<\/b> (da\u011f\u0131t\u0131mc\u0131lar\u0131n rutin olarak atlad\u0131\u011f\u0131 <b>bile\u015fik limit<\/b>) \u00b7 C \u22640,010 \u00b7 Si \u22640,10 \u00b7 Mn \u22643,0 \u00b7 Co \u22643,0 \u00b7 W \u22643,0 \u00b7 Al \u22640,50 \u00b7 Ti \u22640,20 \u00b7 V \u22640,20 \u00b7 Nb \u22640,20 \u00b7 Ta \u22640,20 \u00b7 Cu \u22640,20 \u00b7 Zr \u22640,10 \u00b7 P \u22640,030 \u00b7 S \u22640,010.<\/p>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">ASTM ile EN Ayr\u0131\u015fmalar\u0131 \u2014 Sertifikada Ger\u00e7ekten \u00d6nemli Olanlar<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>S<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>ASTM \u22640,010<\/b> \u00b7 <b>EN\/VdT\u00dcV 517 yolu \u22640,015<\/b>. <b>ASTM daha s\u0131k\u0131d\u0131r.<\/b> S = %0,013&#8217;te EN&#8217;e sertifikal\u0131 bir d\u00f6k\u00fcm <b>ASTM&#8217;de kal\u0131r<\/b>. Sertifikay\u0131 &#8220;B-3&#8243;e kar\u015f\u0131 de\u011fil, <b>m\u00fc\u015fterinin sipari\u015f etti\u011fi \u015fartnameye kar\u015f\u0131<\/b> kontrol edin<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Al<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>ASTM \u22640,50<\/b> \u00b7 bir Avrupa fabrikas\u0131 <b>\u22640,05<\/b> bas\u0131yor \u2014 <b>on kat fark<\/b>, ve patentin <i>tercih etti\u011fi<\/i> Al %0,25\u20130,75 zaten o tavan\u0131n \u00fcst\u00fcnde. B\u00fcy\u00fck olas\u0131l\u0131kla fabrika sayfas\u0131nda ondal\u0131k hatas\u0131; ama yay\u0131mlanm\u0131\u015f. <b>ASTM 0,50&#8217;yi kullan\u0131n ve fark\u0131 dipnot edin<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Zr<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>ASTM tablosu \u22640,10<\/b> \u00b7 \u00fcreticinin kendi nominal tablosu <b>\u22640,01<\/b> \u2014 10 kat fark. Sat\u0131nalma i\u00e7in <b>ASTM 0,10 ge\u00e7erlidir<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Mo \/ Fe \/ Cr (DIN yolu)<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">Bir yay\u0131nc\u0131 DIN 2.4600 i\u00e7in <b>Mo 26\u201332, Fe 1\u20136, Cr 0,5\u20133<\/b> veriyor. Bu <b>tek kaynakl\u0131d\u0131r ve iki Alman fabrikas\u0131 taraf\u0131ndan \u00e7\u00fcr\u00fct\u00fcl\u00fcr<\/b> (ikisi de 27\u201332 \/ 1\u20133 \/ 1\u20133 yay\u0131ml\u0131yor). <b>%6 demir ala\u015f\u0131m-B b\u00f6lgesidir ve korozyon h\u0131z\u0131n\u0131 mahveder \u2014 bunu hata say\u0131n<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Nominal \u2260 \u015fartname<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">\u00dcretici nominali <b>Ni 65 \u00b7 Mo 28,5 \u00b7 Cr 1,5 \u00b7 Fe 1,5<\/b> bir <b>hedef kimyad\u0131r<\/b>. <b>\u015eartname yukar\u0131daki bantlard\u0131r<\/b>, art\u0131 neredeyse hi\u00e7 kimsenin yazmad\u0131\u011f\u0131 <b>Ni+Mo 94\u201398<\/b> bile\u015fik limiti. Fabrika sertifikas\u0131 <b>bantlara kar\u015f\u0131<\/b> denetlenir<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">\u00dc\u00e7 Ku\u015fa\u011f\u0131n Kimyas\u0131 \u2014 Tasar\u0131m Mant\u0131\u011f\u0131 Tek Sat\u0131rda G\u00f6r\u00fcn\u00fcyor<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">C azami<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">Ala\u015f\u0131m B <b>0,05<\/b> \u00b7 B-2 <b>0,02<\/b> \u00b7 <b>B-3 0,010<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Mo<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">26,0\u201330,0 \u00b7 26,0\u201330,0 \u00b7 <b>27,0\u201332,0<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Fe<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>4,0\u20136,0<\/b> \u00b7 \u22642,0 \u00b7 <b>1,0\u20133,0 (ASGAR\u0130 dayat\u0131lm\u0131\u015f)<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Cr<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">\u22641,0 \u00b7 \u22641,0 \u00b7 <b>1,0\u20133,0 (ASGAR\u0130 dayat\u0131lm\u0131\u015f)<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Mn \u00b7 Co \u00b7 V \u00b7 Al<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">Mn \u22641,0 \/ \u22641,0 \/ <b>\u22643,0<\/b> \u00b7 Co \u2014 \/ \u22641,00 \/ \u22643,0 \u00b7 V <b>0,2\u20130,4<\/b> \/ \u2014 \/ \u22640,20 \u00b7 Al \u2014 \/ \u2014 \/ <b>\u22640,50 (bilin\u00e7li)<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Y\u00f6neten kusur<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">M\u2086C karb\u00fcr \u2192 b\u0131\u00e7ak-\u00e7izgisi ata\u011f\u0131 \u00b7 <b>Ni\u2084Mo (\u03b2) d\u00fczenlenme \u2192 gevrekle\u015fme<\/b> \u00b7 <b>Ni\u2083Mo, yava\u015f<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Tasar\u0131m mant\u0131\u011f\u0131<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>B-2, \u03b2 faz\u0131n\u0131 en aza indirmek i\u00e7in Fe ve Cr&#8217;yi a\u015fa\u011f\u0131 \u00e7ekti; B-3 bunu TERS\u0130NE \u00e7evirdi ve her ikisine %1,0 ASGAR\u0130 dayatt\u0131<\/b> \u2014 \u00e7\u00fcnk\u00fc k\u00fc\u00e7\u00fck ve kontroll\u00fc bir yer alan \u00e7\u00f6z\u00fcnen miktar\u0131n\u0131n d\u00fczenlenmeyi <b>te\u015fvik etmek yerine bozdu\u011fu<\/b> ortaya \u00e7\u0131kt\u0131. Ala\u015f\u0131m\u0131n b\u00fct\u00fcn hik\u00e2yesi bu tersine \u00e7evirmedir<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<h4 id=\"dm-b4\" style=\"font-size:19px;font-weight:700;color:#12303f;margin:30px 0 10px;line-height:1.35;\">Mekanik De\u011ferler<\/h4>\n<p><!-- dm-diy-sert --><\/p>\n<div style=\"border:1px solid #e3e9ec;margin:22px 0 26px;background:#fff;position:relative;overflow:hidden;\">\n<div style=\"background:#12303f;color:#fff;padding:9px 14px;font-size:14px;font-weight:700;letter-spacing:.3px;position:relative;z-index:2;\">MUKAVEMET DE\u011eERLER\u0130<\/div>\n<div style=\"position:relative;z-index:2;\">\n<div style=\"padding:12px 10px 0;\"><svg viewBox=\"0 0 740 354\" style=\"width:100%;height:auto;display:block;\" xmlns=\"http:\/\/www.w3.org\/2000\/svg\" role=\"img\"><rect x=\"16\" y=\"6\" width=\"12\" height=\"12\" fill=\"#12303f\"\/><text x=\"34\" y=\"16\" font-size=\"11.5\" fill=\"#12303f\" font-family=\"Arial,Helvetica,sans-serif\">Akma (MPa)<\/text><rect x=\"146\" y=\"6\" width=\"12\" height=\"12\" fill=\"#7fa8bd\"\/><text x=\"164\" y=\"16\" font-size=\"11.5\" fill=\"#12303f\" font-family=\"Arial,Helvetica,sans-serif\">\u00c7ekme (MPa)<\/text><text x=\"16\" y=\"44\" font-size=\"12.5\" font-weight=\"bold\" fill=\"#12303f\" font-family=\"Arial,Helvetica,sans-serif\">ASTM B333 \/ B335 \/ B564 \/ B619 \/ B622 \/ B626 \u00b7 levha, sac, \u015ferit, \u00e7ubuk, d\u00f6vme, b\u2026<\/text><rect x=\"16\" y=\"50\" width=\"559.9\" height=\"15\" fill=\"#7fa8bd\"\/><text x=\"582.9\" y=\"62\" font-size=\"11.5\" fill=\"#5b7180\" font-family=\"Arial,Helvetica,sans-serif\">760<\/text><rect x=\"16\" y=\"68\" width=\"257.9\" height=\"15\" fill=\"#12303f\"\/><text x=\"280.9\" y=\"80\" font-size=\"11.5\" fill=\"#5b7180\" font-family=\"Arial,Helvetica,sans-serif\">350<\/text><text x=\"16\" y=\"108\" font-size=\"12.5\" font-weight=\"bold\" fill=\"#12303f\" font-family=\"Arial,Helvetica,sans-serif\">Avrupa teslim \u015fart\u0131 (Zapp \u00b7 DIN \/ VdT\u00dcV 517)<\/text><rect x=\"16\" y=\"114\" width=\"515.7\" height=\"15\" fill=\"#7fa8bd\"\/><text x=\"538.7\" y=\"126\" font-size=\"11.5\" fill=\"#5b7180\" font-family=\"Arial,Helvetica,sans-serif\">700<\/text><rect x=\"16\" y=\"132\" width=\"239.4\" height=\"15\" fill=\"#12303f\"\/><text x=\"262.4\" y=\"144\" font-size=\"11.5\" fill=\"#5b7180\" font-family=\"Arial,Helvetica,sans-serif\">325<\/text><text x=\"16\" y=\"172\" font-size=\"12.5\" font-weight=\"bold\" fill=\"#12303f\" font-family=\"Arial,Helvetica,sans-serif\">T\u0130P\u0130K \u00b7 levha (Haynes International)<\/text><rect x=\"16\" y=\"178\" width=\"652.0\" height=\"15\" fill=\"#7fa8bd\"\/><text x=\"675.0\" y=\"190\" font-size=\"11.5\" fill=\"#5b7180\" font-family=\"Arial,Helvetica,sans-serif\">885<\/text><rect x=\"16\" y=\"196\" width=\"294.7\" height=\"15\" fill=\"#12303f\"\/><text x=\"317.7\" y=\"208\" font-size=\"11.5\" fill=\"#5b7180\" font-family=\"Arial,Helvetica,sans-serif\">400<\/text><text x=\"16\" y=\"236\" font-size=\"12.5\" font-weight=\"bold\" fill=\"#12303f\" font-family=\"Arial,Helvetica,sans-serif\">T\u0130P\u0130K \u00b7 sac 3,2 mm, parlak tavl\u0131 (Haynes International)<\/text><rect x=\"16\" y=\"242\" width=\"633.6\" height=\"15\" fill=\"#7fa8bd\"\/><text x=\"656.6\" y=\"254\" font-size=\"11.5\" fill=\"#5b7180\" font-family=\"Arial,Helvetica,sans-serif\">860<\/text><rect x=\"16\" y=\"260\" width=\"309.4\" height=\"15\" fill=\"#12303f\"\/><text x=\"332.4\" y=\"272\" font-size=\"11.5\" fill=\"#5b7180\" font-family=\"Arial,Helvetica,sans-serif\">420<\/text><text x=\"16\" y=\"300\" font-size=\"12.5\" font-weight=\"bold\" fill=\"#12303f\" font-family=\"Arial,Helvetica,sans-serif\">T\u0130P\u0130K \u00b7 sac, 538 \u00b0C (1000 \u00b0F)<\/text><rect x=\"16\" y=\"306\" width=\"538.5\" height=\"15\" fill=\"#7fa8bd\"\/><text x=\"561.5\" y=\"318\" font-size=\"11.5\" fill=\"#5b7180\" font-family=\"Arial,Helvetica,sans-serif\">731<\/text><rect x=\"16\" y=\"324\" width=\"203.3\" height=\"15\" fill=\"#12303f\"\/><text x=\"226.3\" y=\"336\" font-size=\"11.5\" fill=\"#5b7180\" font-family=\"Arial,Helvetica,sans-serif\">276<\/text><\/svg><\/div>\n<div style=\"padding:12px 12px 2px;position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"overflow-x:auto;position:relative;z-index:2;\">\n<table style=\"width:100%;border-collapse:collapse;font-size:13.5px;min-width:430px;background:transparent;\">\n<tr>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">Ko\u015ful<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">Sertlik<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">Akma MPa<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">\u00c7ekme MPa<\/th>\n<th style=\"padding:7px 9px;text-align:left;font-size:12px;color:#12303f;background:#F2F6F8;border:1px solid #eceff1;\">Uzama<\/th>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">ASTM B333 \/ B335 \/ B564 \/ B619 \/ B622 \/ B626 \u00b7 levha, sac, \u015ferit, \u00e7ubuk, d\u00f6vme, boru, t\u00fcp<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">\u2014<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">350<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">760<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">%40<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">Avrupa teslim \u015fart\u0131 (Zapp \u00b7 DIN \/ VdT\u00dcV 517)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">\u2014<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">325-340<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">700-1000<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">%40<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">T\u0130P\u0130K \u00b7 levha (Haynes International)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">95 HRBW<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">400<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">885<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">%57,8<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">T\u0130P\u0130K \u00b7 sac 3,2 mm, parlak tavl\u0131 (Haynes International)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">93 HRBW<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">420<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">860<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">%53,4<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;\">T\u0130P\u0130K \u00b7 \u00e7ubuk (Haynes International)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">92 HRBW<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">\u2014<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">\u2014<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">\u2014<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;\">T\u0130P\u0130K \u00b7 sac, 538 \u00b0C (1000 \u00b0F)<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">\u2014<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">276<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">731<\/td>\n<td style=\"padding:7px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">%62<\/td>\n<\/tr>\n<\/table>\n<\/div>\n<\/div>\n<\/div>\n<div style=\"padding:6px 14px 12px;font-size:12px;color:#5b7180;line-height:1.7;border-top:1px solid #f0f3f5;position:relative;z-index:2;\"><b style=\"color:#12303f;\">\u0130LK SATIR ASTM \u015eARTNAME M\u0130N\u0130MUMUDUR ve oda s\u0131cakl\u0131\u011f\u0131 i\u00e7indir; B333, B335, B564, B619, B622 ve B626 N10675 i\u00e7in AYNI minimum seti ta\u015f\u0131d\u0131\u011f\u0131ndan tek sat\u0131rda toplanm\u0131\u015ft\u0131r. \u0130K\u0130NC\u0130 SATIR Avrupa (Zapp, DIN\/VdT\u00dcV 517) teslim \u015fart\u0131d\u0131r. SON D\u00d6RT SATIR \u00fcretici T\u0130P\u0130K de\u011feridir, \u015fartname \u015fart\u0131 DE\u011e\u0130LD\u0130R; hesaba tipik de\u011fer konmaz. N10675 \u00c7\u00d6KELME SERTLE\u015eMED\u0130\u011e\u0130 \u0130\u00c7\u0130N sat\u0131rlar ya\u015fland\u0131rma ko\u015fuluna g\u00f6re de\u011fil \u015eARTNAME ve \u00dcR\u00dcN FORMUNA g\u00f6re ayr\u0131lm\u0131\u015ft\u0131r; H900 \/ H1075 benzeri bir ko\u015ful s\u00fctunu YOKTUR. AMS SATIRI YOKTUR: N10675 i\u00e7in do\u011frulanm\u0131\u015f AMS \u015fartnamesi bulunamam\u0131\u015ft\u0131r.<\/b> Grafikte aral\u0131k olarak verilen de\u011ferler alt s\u0131n\u0131rdan \u00e7izilmi\u015ftir; tam aral\u0131k tablodad\u0131r. \u015eARTNAME M\u0130N\u0130MUMU \u0130LE T\u0130P\u0130K DE\u011eER AYRI TUTULMU\u015eTUR. Hesaba yaln\u0131zca minimum girer. \u00c7EKME DAYANIMI 760 MPa M\u0130N\u0130MUM, C ailesinin 690 MPa minimumundan Y\u00dcKSEKT\u0130R; buna kar\u015f\u0131l\u0131k uzama minimumu %40&#8217;t\u0131r (C-276 ve C-22&#8217;de %45). Bu fark ala\u015f\u0131m\u0131n y\u00fcksek molibden i\u00e7eri\u011finden gelir. SERTL\u0130K YALNIZCA HRB C\u0130NS\u0130NDEN VER\u0130LM\u0130\u015eT\u0130R; bu ala\u015f\u0131m i\u00e7in HRC anlaml\u0131 de\u011fildir (\u00e7\u00f6zelti tavl\u0131 durumda 92-95 HRBW). 538 \u00b0C sat\u0131r\u0131 bir kod de\u011feri DE\u011e\u0130LD\u0130R: ASME B\u00f6l\u00fcm VIII Div. 1 ve B31.3 tavan\u0131 427 \u00b0C&#8217;dir.<\/div>\n<\/div>\n<p><!-- \/dm-diy-sert --><\/p>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">\u015eartname Asgarileri \u2014 \u0130ki Ayr\u0131 Sistem, Sat\u0131rlar\u0131 KARI\u015eTIRMAYIN<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>ASTM yolu<\/b> (B333\/B335\/B619\/B622\/B626), \u00e7\u00f6zelti tavl\u0131<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">\u00c7ekme <b>\u2265760 MPa (110 ksi)<\/b> \u00b7 Rp0,2 <b>\u2265350 MPa (51 ksi)<\/b> \u00b7 Uzama (50 mm) <b>\u2265%40<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>EN \/ VdT\u00dcV 517<\/b> \u2014 sac ve levha \u226465 mm<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">Rp0,2 <b>\u2265340 MPa<\/b> \u00b7 Rp1,0 <b>\u2265380 MPa<\/b> \u00b7 Rm <b>700\u20131000 MPa<\/b> \u00b7 A <b>\u2265%40<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>EN \/ VdT\u00dcV 517<\/b> \u2014 d\u00f6vme ve bar \u226490 mm<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">Rp0,2 <b>\u2265325 MPa<\/b> \u00b7 Rm <b>700\u2013950 MPa<\/b> \u00b7 A <b>\u2265%40<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>EN&#8217;de Rm bir BANTTIR<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">ASTM yaln\u0131zca taban koyar (760 MPa); <b>EN 700\u20131000 MPa&#8217;l\u0131k bir tavan da koyar<\/b>. <b>\u00c7ok y\u00fcksek dayan\u0131ml\u0131 bir d\u00f6k\u00fcm ASTM&#8217;yi ge\u00e7ip EN&#8217;de kalabilir.<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>S\u0131k yap\u0131lan hata<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">Bir sayfa <b>ASTM \u00e7ekmesini (760 MPa)<\/b> ile <b>EN akmas\u0131n\u0131 (340 MPa)<\/b> ayn\u0131 tabloda e\u015fle\u015ftiriyor. <b>Bu sat\u0131r hi\u00e7bir standartta yoktur.<\/b> ASTM = 760\/350\/%40; EN = 700\u20131000\/340\/%40<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">EN y\u00fcksek s\u0131cakl\u0131k Rp0,2 asgarileri<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">Sac\/levha: 100 \u00b0C <b>315<\/b> \u00b7 200 \u00b0C <b>285<\/b> \u00b7 300 \u00b0C <b>270<\/b> \u00b7 400 \u00b0C <b>255 MPa<\/b> \u00b7 D\u00f6vme\/bar: 300 \u00b7 275 \u00b7 255 \u00b7 <b>240 MPa<\/b>. VdT\u00dcV yolunda tasar\u0131m hesab\u0131n\u0131n kulland\u0131\u011f\u0131 de\u011ferler bunlard\u0131r<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">Tipik Fabrika De\u011ferleri \u2014 GARANT\u0130 DE\u011e\u0130L<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Sac 3,2 mm (Rp0,2 \/ Rm \/ A)<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">OS <b>421 \/ 862 MPa \/ %53<\/b> \u00b7 93 \u00b0C 379\/834\/%57 \u00b7 204 \u00b0C 324\/758\/%60 \u00b7 316 \u00b0C 303\/717\/%63 \u00b7 427 \u00b0C 290\/703\/%62 \u00b7 538 \u00b0C 269\/676\/%59 \u00b7 <b>649 \u00b0C 317\/717\/%56<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Levha (Rp0,2 \/ Rm \/ A)<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">OS <b>400 \/ 883 MPa \/ %58<\/b> \u00b7 204 \u00b0C 331\/793\/%61 \u00b7 427 \u00b0C 283\/745\/%62 \u00b7 538 \u00b0C 276\/731\/%62 \u00b7 <b>649 \u00b0C 290\/738\/%65<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>538 \u2192 649 \u00b0C aras\u0131ndaki Y\u00dcKSEL\u0130\u015e<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>\u00d6l\u00e7\u00fcm hatas\u0131 de\u011fildir.<\/b> Bir Ni-Mo kat\u0131 \u00e7\u00f6zeltisinde <b>k\u0131sa menzilli d\u00fczenlenmenin ba\u015flad\u0131\u011f\u0131n\u0131n klasik imzas\u0131d\u0131r<\/b> \u2014 ve ala\u015f\u0131m\u0131 orada kullanmaya bir davet <b>de\u011fildir<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Sertlik ve tane boyutu<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">Sac <b>93 HRBW<\/b> (tane 4,5\u20136,5) \u00b7 levha <b>95 HRBW<\/b> (3,5\u20137) \u00b7 bar <b>92 HRBW<\/b> (2\u20137,5). <b>92\u201395 HRB kabaca 15\u201317 HRC&#8217;dir<\/b> \u2014 her 22 HRC e\u015fi\u011finin \u00e7ok alt\u0131nda. <b>\u00d6l\u00e7e\u011fi daima yaz\u0131n<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Charpy V-\u00e7entik<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">Levha 20 mm: OS <b>479 J<\/b>, \u2212196 \u00b0C <b>453 J<\/b> \u00b7 levha 35 mm: 526 \/ 487 J \u00b7 bar 40 mm: 526 \/ 460 J \u00b7 bar 50 mm: <b>529 \/ 458 J<\/b>. <b>\u2212196 \u00b0C&#8217;ye kadar fiilen s\u00fcnek\u2013gevrek ge\u00e7i\u015f yoktur<\/b> \u2014 kriyojenik al\u0131c\u0131ya s\u00f6ylenmeye de\u011fer<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<h4 id=\"dm-b5\" style=\"font-size:19px;font-weight:700;color:#12303f;margin:30px 0 10px;line-height:1.35;\">Fiziksel \u00d6zellikler<\/h4>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">Fiziksel \u00d6zellikler \u00b7 Hastelloy B-3<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Yo\u011funluk<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>9,22 g\/cm\u00b3<\/b> (0,333 lb\/in\u00b3) \u2014 d\u00f6rt ba\u011f\u0131ms\u0131z yay\u0131nc\u0131. <b>9,13 ve 9,3 ayk\u0131r\u0131 de\u011ferleri vard\u0131r; 9,22 kullan\u0131n<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Ergime aral\u0131\u011f\u0131<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>1370\u20131418 \u00b0C<\/b> (2500\u20132585 \u00b0F)<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Elastisite mod\u00fcl\u00fc<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>216\u2013217 GPa<\/b>. S\u0131cakl\u0131kla: 204 \u00b0C 208 \u00b7 316 \u00b0C 202 \u00b7 427 \u00b0C 195 \u00b7 538 \u00b0C 188 \u00b7 649 \u00b0C 183 GPa<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Is\u0131 iletkenli\u011fi, OS<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>11,2 W\/m\u00b7K<\/b>. S\u0131cakl\u0131kla: 204 \u00b0C 13,4 \u00b7 316 \u00b0C 15,0 \u00b7 427 \u00b0C 16,7 \u00b7 538 \u00b0C 18,6 \u00b7 649 \u00b0C 20,5 W\/m\u00b7K<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Ortalama \u0131s\u0131l genle\u015fme<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>10,6 \u00d7 10\u207b\u2076 \/K<\/b> (25\u2013100 \u00b0C). 25\u2013316 \u00b0C 11,3 \u00b7 25\u2013538 \u00b0C 11,9<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Elektriksel \u00f6zdiren\u00e7<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>1,37 \u00b5\u03a9\u00b7m<\/b> (137 \u00b5\u03a9\u00b7cm). <b>S\u0131cakl\u0131kla neredeyse sabittir<\/b> \u2014 deri\u015fik bir kat\u0131 \u00e7\u00f6zeltinin tipik davran\u0131\u015f\u0131<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">\u00d6zg\u00fcl \u0131s\u0131, OS<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>373 J\/kg\u00b7K<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Poisson \u00b7 kayma mod\u00fcl\u00fc<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">0,31 \u00b7 85 GPa \u2014 <b>yaln\u0131zca ikincil veri taban\u0131<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Manyetiklik<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">Tek fazl\u0131 YMK (\u03b3) ostenitik kat\u0131 \u00e7\u00f6zelti, dolay\u0131s\u0131yla \u00e7\u00f6zelti tavl\u0131 h\u00e2lde <b>paramanyetik \/ fiilen manyetik de\u011fil<\/b>. <b>Say\u0131sal bir ba\u011f\u0131l ge\u00e7irgenlik de\u011feri bulunamad\u0131 \u2014 bir \u00b5r rakam\u0131 yay\u0131mlamay\u0131n<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Ticari olarak anlaml\u0131 nokta<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>11,2 W\/m\u00b7K<\/b> karbon \u00e7eli\u011finin kabaca d\u00f6rtte biri, 316L&#8217;nin ~%70&#8217;i; <b>10,6 \u00d7 10\u207b\u2076\/K<\/b> ise 316L&#8217;nin ~16&#8217;s\u0131n\u0131n <b>\u00fc\u00e7te ikisi<\/b>. B-3 boru aynas\u0131 veya B-3 kaplamal\u0131 kap i\u00e7in bu, paslanmaz kaplamaya g\u00f6re <b>karbon \u00e7eli\u011fine kar\u015f\u0131 daha az diferansiyel genle\u015fme<\/b> demektir \u2014 ger\u00e7ek bir tasar\u0131m avantaj\u0131 ve neredeyse hi\u00e7bir da\u011f\u0131t\u0131mc\u0131 sayfas\u0131 yazm\u0131yor<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<h4 id=\"dm-b6\" style=\"font-size:19px;font-weight:700;color:#12303f;margin:30px 0 10px;line-height:1.35;\">Is\u0131l \u0130\u015flem ve Is\u0131l Kararl\u0131l\u0131k<\/h4>\n<p><!-- dm-diy-isil --><\/p>\n<div style=\"border:1px solid #e3e9ec;margin:22px 0 26px;background:#fff;position:relative;overflow:hidden;\">\n<div style=\"background:#12303f;color:#fff;padding:9px 14px;font-size:14px;font-weight:700;letter-spacing:.3px;position:relative;z-index:2;\">ISIL \u0130\u015eLEM \u2014 \u015eEMAT\u0130K<\/div>\n<div style=\"position:relative;z-index:2;\">\n<div style=\"padding:10px 12px 2px;position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"position:relative;z-index:2;\">\n<div style=\"font-size:13.5px;font-weight:700;color:#12303f;margin:6px 0 6px;\">\u00c7\u00d6ZELT\u0130 TAVI (solution anneal) \u2014 tek ge\u00e7erli \u0131s\u0131l i\u015flem budur<\/div>\n<table style=\"width:100%;border-collapse:collapse;font-size:13.5px;background:transparent;\">\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">Ad\u0131m<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">\u00c7\u00d6ZELT\u0130 TAVI (solution anneal) \u2014 tek ge\u00e7erli \u0131s\u0131l i\u015flem budur<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">\u00d6zet<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">Ala\u015f\u0131m\u0131n tek \u0131s\u0131l i\u015flemi. So\u011fuk i\u015flemi geri al\u0131r, \u00e7\u00f6keltileri kat\u0131 \u00e7\u00f6zeltiye sokar, korozyon direncini ve s\u00fcnekli\u011fi geri kazand\u0131r\u0131r. Dayan\u0131m\u0131 ARTIRMAZ; d\u00fc\u015f\u00fcr\u00fcr. Teslim durumu budur.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">S\u0131cakl\u0131k<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Haynes International 1066 \u00b0C (1950 \u00b0F), tolerans \u00b114 \u00b0C (\u00b125 \u00b0F) \u00b7 Corrosion Materials 1065 \u00b0C (1950 \u00b0F) \u00b7 Virgamet 1060 \u00b0C \u00b7 Zapp 1050-1080 \u00b0C. Toplu bant: 1050-1080 \u00b0C.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">S\u00fcre<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">Haynes International kal\u0131nl\u0131\u011fa g\u00f6re 10-30 dakika verir. Di\u011fer kaynaklar s\u00fcre vermedi\u011fi i\u00e7in tek bir say\u0131 yaz\u0131lmam\u0131\u015ft\u0131r.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">So\u011futma<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">HIZLI SO\u011eUTMA ZORUNLUDUR. Haynes International: su verme tercih edilir, 9,5 mm \u00fczeri kesitte \u00f6zellikle tavsiye edilir; ince kesitte h\u0131zl\u0131 hava so\u011futma kabul edilir; f\u0131r\u0131ndan \u00e7\u0131k\u0131\u015f ile su vermenin ba\u015flamas\u0131 aras\u0131ndaki s\u00fcre 3 DAK\u0130KADAN AZ olmal\u0131d\u0131r. Zapp: su, bas\u0131n\u00e7l\u0131 hava veya koruyucu gaz. Virgamet: su veya h\u0131zl\u0131 hava so\u011futma. Gerek\u00e7e (Haynes International): yava\u015f so\u011fuma tane s\u0131n\u0131rlar\u0131nda zararl\u0131 ikincil faz \u00e7ekirdeklenmesine ve b\u00fcy\u00fcmesine yol a\u00e7ar.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">Ne i\u00e7in<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">Teslim durumu; her s\u0131cak \u015fekillendirmeden sonra; d\u0131\u015f lif uzamas\u0131 %7&#8217;yi a\u015fan her so\u011fuk \u015fekillendirmeden sonra (kaynak yap\u0131lacaksa); ara s\u0131cakl\u0131kta kalm\u0131\u015f par\u00e7ay\u0131 kurtarmak i\u00e7in. ASTM B333 \/ B335 \/ B564 \/ B619 \/ B622 \/ B626 malzemeyi \u00e7\u00f6zelti tavl\u0131 ve tufalsiz ister.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">Sonu\u00e7 sertlik<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Tavlanm\u0131\u015f durumda Haynes International levha ve \u00e7ubuk i\u00e7in 92-95 HRBW bildirir. Bu bir hedef de\u011fil, teslim durumunun tipik sonucudur.<\/td>\n<\/tr>\n<\/table>\n<\/div>\n<\/div>\n<div style=\"padding:10px 12px 2px;position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"position:relative;z-index:2;\">\n<div style=\"font-size:13.5px;font-weight:700;color:#12303f;margin:6px 0 6px;\">PARLAK TAVLAMA (bright anneal) \u2014 yaln\u0131zca ince sac ve \u015ferit i\u00e7in<\/div>\n<table style=\"width:100%;border-collapse:collapse;font-size:13.5px;background:transparent;\">\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">Ad\u0131m<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">PARLAK TAVLAMA (bright anneal) \u2014 yaln\u0131zca ince sac ve \u015ferit i\u00e7in<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">\u00d6zet<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">\u0130nce sac ve bobin \u00fcr\u00fcnlerde y\u00fczeyi tufalsiz b\u0131rakmak i\u00e7in kullan\u0131lan ayr\u0131 bir kol. \u00c7\u00f6zelti tav\u0131n\u0131n yerini tutar ancak s\u0131cakl\u0131\u011f\u0131 daha y\u00fcksektir.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">S\u0131cakl\u0131k<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">1150 \u00b0C (2100 \u00b0F) \u2014 Corrosion Materials ve Elgiloy.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">S\u00fcre<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">Kaynaklar s\u00fcre vermez; yaz\u0131lmam\u0131\u015ft\u0131r.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">So\u011futma<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Hidrojen atmosferinde so\u011futma (Corrosion Materials, Elgiloy).<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">Ne i\u00e7in<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">Parlak tavl\u0131 sac ve bobin teslimi. Bu koldan \u00e7\u0131kan 3,2 mm sac i\u00e7in bildirilen tipik de\u011ferler: 860 MPa \u00e7ekme, 420 MPa akma, %53,4 uzama.<\/td>\n<\/tr>\n<\/table>\n<\/div>\n<\/div>\n<div style=\"padding:10px 12px 2px;position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"position:relative;z-index:2;\">\n<div style=\"font-size:13.5px;font-weight:700;color:#12303f;margin:6px 0 6px;\">SICAK \u015eEK\u0130LLEND\u0130RME (hot working) \u2014 \u0131s\u0131l i\u015flem de\u011fil, \u015fekillendirme penceresi<\/div>\n<table style=\"width:100%;border-collapse:collapse;font-size:13.5px;background:transparent;\">\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">Ad\u0131m<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">SICAK \u015eEK\u0130LLEND\u0130RME (hot working) \u2014 \u0131s\u0131l i\u015flem de\u011fil, \u015fekillendirme penceresi<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">\u00d6zet<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">Aral\u0131k dard\u0131r; a\u015f\u0131l\u0131rsa \u00e7atlak \u00fcretir. Sonras\u0131nda \u00e7\u00f6zelti tav\u0131 zorunludur.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">S\u0131cakl\u0131k<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Ba\u015flang\u0131\u00e7 1232 \u00b0C (2250 \u00b0F), biti\u015f 982 \u00b0C (1800 \u00b0F) \u2014 Haynes International. Virgamet 1230-980 \u00b0C verir.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">S\u00fcre<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">\u2014<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">So\u011futma<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">\u015eekillendirme sonras\u0131 \u00e7\u00f6zelti tav\u0131 ve h\u0131zl\u0131 so\u011futma uygulan\u0131r.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">Ne i\u00e7in<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">D\u00f6vme ve s\u0131cak haddeleme.<\/td>\n<\/tr>\n<\/table>\n<\/div>\n<\/div>\n<div style=\"padding:10px 12px 2px;position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"position:relative;z-index:2;\">\n<div style=\"font-size:13.5px;font-weight:700;color:#12303f;margin:6px 0 6px;\">Ka\u00e7\u0131n\u0131lacak b\u00f6lge<\/div>\n<table style=\"width:100%;border-collapse:collapse;font-size:13.5px;background:transparent;\">\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">Ad\u0131m<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">ARA SICAKLIK BANDI \u2014 bu bir sertle\u015ftirme \u00e7evrimi DE\u011e\u0130LD\u0130R, ka\u00e7\u0131n\u0131lacak b\u00f6lgedir<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">S\u0131cakl\u0131k<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">TEK BANT YAZILMAMI\u015eTIR; 4 ba\u011f\u0131ms\u0131z kaynakla do\u011frulanamam\u0131\u015ft\u0131r. Bulunanlar kaynak ad\u0131yla: Haynes International (\u0131s\u0131l i\u015flem k\u0131lavuzu) 593-816 \u00b0C (1100-1500 \u00b0F) \u2014 so\u011fuk i\u015flenmi\u015f B-3&#8217;\u00fcn bu bantta bekletilmemesi istenir, tavlama \u00f6n \u0131s\u0131t\u0131lm\u0131\u015f f\u0131r\u0131nda yap\u0131l\u0131r \u00b7 Haynes International (B-3 bro\u015f\u00fcr\u00fc) T-T-T kar\u015f\u0131la\u015ft\u0131rmas\u0131n\u0131 700 \u00b0C (1290 \u00b0F) \u00fczerinden verir \u00b7 Huaxiao 550-850 \u00b0C band\u0131n\u0131 ara s\u0131cakl\u0131k gevrekle\u015fmesi olarak bildirir. Bu \u00fc\u00e7 kay\u0131t iki kurulu\u015ftan gelmektedir; bu y\u00fczden karta SAYISAL B\u0130R YASAK BANT OLARAK KONMAMI\u015eTIR.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">Sonu\u00e7<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">Bu bantta uzun s\u00fcre tutulan malzemede s\u00fcneklik ve darbe toklu\u011fu d\u00fc\u015fer. Kurtarma yolu tek: tam \u00e7\u00f6zelti tav\u0131 + h\u0131zl\u0131 so\u011futma.<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">Fazlar<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(247,250,251,.78);color:#3d5260;\">Ni4Mo ve Ni3Mo. Haynes International&#8217;\u0131n ifadesi: B-2 ala\u015f\u0131m\u0131 750 \u00b0C dolay\u0131nda HIZLA Ni4Mo olu\u015fturur; B-3&#8217;te ise k\u00fc\u00e7\u00fck ala\u015f\u0131m ilaveleri ve ayarlanm\u0131\u015f molibden ile YAVA\u015e olu\u015fan Ni3Mo tercih edilmi\u015ftir ve zararl\u0131 faz\u0131n geli\u015fmesi 650 \u00b0C dolay\u0131nda saatler al\u0131r. Bu, B-3&#8217;\u00fcn B-2&#8217;den ayr\u0131ld\u0131\u011f\u0131 as\u0131l noktad\u0131r.<\/td>\n<\/tr>\n<\/table>\n<\/div>\n<\/div>\n<div style=\"padding:10px 12px 2px;position:relative;overflow:hidden;\"><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<div style=\"position:relative;z-index:2;\">\n<div style=\"font-size:13.5px;font-weight:700;color:#12303f;margin:6px 0 6px;\">Ek bilgiler<\/div>\n<table style=\"width:100%;border-collapse:collapse;font-size:13.5px;background:transparent;\">\n<tr>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);font-weight:700;color:#12303f;width:34%;vertical-align:top;\">Yap\u0131lmamas\u0131 gereken i\u015flemler<\/td>\n<td style=\"padding:6px 9px;border:1px solid #eceff1;background:rgba(255,255,255,.72);color:#3d5260;\">YA\u015eLANDIRMA \/ \u00c7\u00d6KELME SERTLE\u015eT\u0130RME: b\u00f6yle bir kademe YOKTUR. H900, H1025, H1075, H1150 benzeri ko\u015fullar bu ala\u015f\u0131ma ait de\u011fildir. \u00b7 \u00c7\u00d6ZELT\u0130 TAVI SONRASI YAVA\u015e SO\u011eUTMA (f\u0131r\u0131nda veya sakin havada, kal\u0131n kesitte): i\u015flemi ge\u00e7ersiz k\u0131lar; tane s\u0131n\u0131rlar\u0131nda ikincil faz \u00e7ekirdeklenir. \u00b7 SO\u011eUK FIRINA \u015eARJ: par\u00e7a \u00f6n \u0131s\u0131t\u0131lm\u0131\u015f f\u0131r\u0131na verilir; yava\u015f \u0131s\u0131nma ara s\u0131cakl\u0131k band\u0131nda gereksiz s\u00fcre ge\u00e7irtir (Haynes International). \u00b7 427 \u00b0C \u00dcZER\u0130NDE KOD SERV\u0130S\u0130: ASME B\u00f6l\u00fcm VIII Div. 1 ve B31.3 tavan\u0131 427 \u00b0C&#8217;dir; ASME B\u00f6l\u00fcm XII i\u00e7in 343 \u00b0C.<\/td>\n<\/tr>\n<\/table>\n<\/div>\n<\/div>\n<\/div>\n<div style=\"padding:6px 14px 12px;font-size:12px;color:#5b7180;line-height:1.7;border-top:1px solid #f0f3f5;position:relative;z-index:2;\">\u015eema \u015fematiktir; zaman ekseni \u00f6l\u00e7ekli de\u011fildir. Hastelloy B-3 KATI \u00c7\u00d6ZELT\u0130 ala\u015f\u0131m\u0131d\u0131r ve \u00c7\u00d6KELME SERTLE\u015eMEZ \u2014 ya\u015fland\u0131rma kademesi YOKTUR, bu y\u00fczden ya\u015fland\u0131rma diyagram\u0131 \u00e7izilmemi\u015ftir. Haynes International&#8217;\u0131n yay\u0131mlad\u0131\u011f\u0131 T-T-T kar\u015f\u0131la\u015ft\u0131rmas\u0131 bu karta E\u011eR\u0130 olarak aktar\u0131lmam\u0131\u015ft\u0131r; e\u011frinin say\u0131sal noktalar\u0131 4 ba\u011f\u0131ms\u0131z kaynakla okunamam\u0131\u015ft\u0131r. \u015eema \u015fematiktir; zaman ekseni \u00f6l\u00e7ekli de\u011fildir. Yay\u0131mlanm\u0131\u015f TTT\/CCT e\u011frisinin say\u0131sal noktalar\u0131 4 ba\u011f\u0131ms\u0131z kaynakla okunamad\u0131\u011f\u0131 i\u00e7in e\u011fri \u00e7izilmemi\u015ftir. Hastelloy B-3 KATI \u00c7\u00d6ZELT\u0130 ala\u015f\u0131m\u0131d\u0131r. Ya\u015fland\u0131rma kademesi YOKTUR; sertlik yaln\u0131zca so\u011fuk \u015fekillendirmeyle artar ve \u00e7\u00f6zelti tav\u0131 ile geri al\u0131n\u0131r. PARLAK TAVLAMA \u0130LE \u00c7\u00d6ZELT\u0130 TAVI AYNI \u015eEY DE\u011e\u0130LD\u0130R: 1150 \u00b0C hidrojen so\u011futmal\u0131 parlak tavlama ince sac ve bobin kolu, 1066 \u00b0C su verme ise genel \u00e7\u00f6zelti tav\u0131 koludur. Sipari\u015f metninde hangisinin istendi\u011fi ayr\u0131ca yaz\u0131lmal\u0131d\u0131r. \u00c7\u00d6ZELT\u0130 TAVI \u0130\u00c7\u0130N S\u00dcRE TEK SAYIYLA VER\u0130LMEM\u0130\u015eT\u0130R: yaln\u0131zca Haynes International (10-30 dakika) s\u00fcre vermektedir.<\/div>\n<\/div>\n<p><!-- \/dm-diy-isil --><\/p>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">\u00c7\u00f6zelti Tav\u0131<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>\u00dcretici \/ ASTM yolu<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>1066 \u00b0C (1950 \u00b0F)<\/b>, kal\u0131nl\u0131\u011fa g\u00f6re <b>10\u201330 dakika<\/b> (a\u011f\u0131r kesitte tam 30 dak). <b>Su verme tavsiye edilir<\/b>; <b>&lt;10 mm (0,375 in\u00e7)<\/b> kesitlerde h\u0131zl\u0131 hava so\u011futmas\u0131 kabul edilebilir<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Parlak tav (sac\/rulo)<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>1150 \u00b0C (2100 \u00b0F)<\/b>, <b>hidrojen<\/b> i\u00e7inde so\u011futma<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>EN \/ VdT\u00dcV yolu<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>1050\u20131080 \u00b0C<\/b>, <b>h\u0131zl\u0131 su verme<\/b> \u2014 su, bas\u0131n\u00e7l\u0131 hava veya koruyucu gaz<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>\u0130ki yol \u00e7eli\u015fmiyor<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">1066 \u00b0C, EN&#8217;in 1050\u20131080 \u00b0C band\u0131n\u0131n <b>i\u00e7indedir<\/b>. \u0130ki rakam bas\u0131p okuyucuyu tahmine b\u0131rakmak yerine <b>bunu a\u00e7\u0131k\u00e7a yaz\u0131n<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Su verme iste\u011fe ba\u011fl\u0131 DE\u011e\u0130LD\u0130R<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">Tav\u0131n b\u00fct\u00fcn amac\u0131 <b>d\u00fczensiz \u03b3 kat\u0131 \u00e7\u00f6zeltisini dondurmakt\u0131r<\/b>. 900\u2192500 \u00b0C aras\u0131nda f\u0131r\u0131n so\u011futmas\u0131, tav\u0131n gidermek i\u00e7in yap\u0131ld\u0131\u011f\u0131 sorunu <b>yeniden yarat\u0131r<\/b>. \u00dcretici rehberi: &#8220;h\u0131zl\u0131 \u0131s\u0131tma, hassas s\u0131cakl\u0131k kontrol\u00fc, h\u0131zl\u0131 so\u011futma&#8221;<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">Is\u0131l Kararl\u0131l\u0131k \/ Gevrekle\u015fme Penceresi \u2014 Kaynaklar Ayr\u0131\u015f\u0131yor<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">\u00dcretici bro\u015f\u00fcr\u00fc<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>500\u2013900 \u00b0C<\/b> \u2014 &#8220;istenen YMK gama faz\u0131 d\u0131\u015f\u0131ndaki fazlar\u0131n olu\u015fmas\u0131 i\u00e7in g\u00fc\u00e7l\u00fc bir e\u011filim\u2026 \u00f6zellikle 500\u2013900 \u00b0C aral\u0131\u011f\u0131nda&#8221;<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Alman fabrika 1<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>500\u2013820 \u00b0C<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Alman fabrika 2<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>500\u2013800 \u00b0C<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Patent<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">D\u00fczenli Ni\u2082Mo\/Ni\u2083Mo\/Ni\u2084Mo fazlar\u0131 i\u00e7in \u00f6zellikle <b>600\u2013800 \u00b0C<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Nas\u0131l yay\u0131mlanmal\u0131<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>T\u00fcm kaynaklar alt s\u0131n\u0131r\u0131n ~500 \u00b0C oldu\u011funda hemfikirdir.<\/b> \u00dcst s\u0131n\u0131r 800\u2013900 \u00b0C aras\u0131nda veriliyor; <b>\u00e7o\u011funluk 800\u2013820 \u00b0C&#8217;de<\/b>, \u00fcretici en geni\u015f ve en muhafazak\u00e2r 900 \u00b0C&#8217;yi veriyor. <b>Muhafazak\u00e2r zarf\u0131 yaz\u0131n: &#8220;500\u2013900 \u00b0C aras\u0131nda s\u00fcrekli maruziyetten ka\u00e7\u0131n\u0131n&#8221;<\/b> ve Avrupa fabrika sayfalar\u0131n\u0131n 500\u2013800\/820 \u00b0C dedi\u011fini dipnot edin. <b>Asla ortalamas\u0131n\u0131 al\u0131p 850 demeyin<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Pencere i\u00e7indeki kinetik<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">B-3 e\u011frisinin burnu <b>~650 \u00b0C<\/b>&#8216;dedir ve orada zararl\u0131 ikincil faz i\u00e7in <b>birka\u00e7 saat<\/b> gerekir \u00b7 B-2 kar\u015f\u0131la\u015ft\u0131rmas\u0131: <b>~750 \u00b0C&#8217;de h\u0131zl\u0131 Ni\u2084Mo<\/b>, <b>700 \u00b0C&#8217;de 0,5\u20131,0 saatte 10+ HRA<\/b> \u00b7 B-3 <b>700 \u00b0C&#8217;de 24 saat: kayda de\u011fer sertle\u015fme yok<\/b> \u00b7 B-3 <b>540 \u00b0C&#8217;de 16.000 saat: uzama h\u00e2l\u00e2 %43,7<\/b>. <b>~540 \u00b0C alt\u0131nda zaman, pratik tesis \u00f6mr\u00fc i\u00e7in fiilen bir fakt\u00f6r de\u011fildir<\/b><\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">S\u0131cak ve So\u011fuk \u0130\u015fleme<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">S\u0131cak i\u015fleme aral\u0131\u011f\u0131<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>1232 \u00b0C \u2192 982 \u00b0C (2250\u20131800 \u00b0F)<\/b>. \u00dcretici: s\u0131cak i\u015fleme &#8220;<b>dar bir s\u0131cakl\u0131k aral\u0131\u011f\u0131 ve s\u0131k yeniden \u0131s\u0131tma<\/b> gerektirir&#8221; \u2014 paslanmaz bir i\u015fe g\u00f6re <b>daha fazla yeniden \u0131s\u0131tma b\u00fct\u00e7eleyin<\/b>. <b>T\u00fcm s\u0131cak \u015fekillendirmeden sonra yeniden tavlay\u0131n<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">So\u011fuk i\u015fleme<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">B-3 <b>ostenitik paslanmazdan daha h\u0131zl\u0131 pekle\u015fir<\/b>. Ara tavlar\u0131 ve pres tonaj\u0131n\u0131 ona g\u00f6re boyutland\u0131r\u0131n<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Yeniden tav e\u015fi\u011fi \u2014 ayr\u0131\u015fma<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>\u00dcretici: d\u0131\u015f lif uzamas\u0131 ~%7&#8217;yi a\u015farsa<\/b> ileri imalat\/kaynaktan \u00f6nce \u00e7\u00f6zelti tav\u0131 gerekir \u2014 &#8220;optimum korozyon ba\u015far\u0131m\u0131 i\u00e7in&#8221; ve \u00e7\u00fcnk\u00fc so\u011fuk i\u015f giderilmezse <b>&#8220;B-3 sonraki imalat\/kaynak s\u0131ras\u0131nda kaynak b\u00f6lgesinde \u00e7atlamaya \u00e7ok yatk\u0131nd\u0131r&#8221;<\/b> \u00b7 <b>Bir Avrupa fabrikas\u0131: %15<\/b>. <b>\u00c7o\u011funluk ve fabrikan\u0131n kendi rakam\u0131 %7&#8217;dir; %7&#8217;yi \u00e7al\u0131\u015fma kural\u0131 yap\u0131n<\/b>, \u00f6zellikle HCl servisine girecek her \u015feyde<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<h4 id=\"dm-b7\" style=\"font-size:19px;font-weight:700;color:#12303f;margin:30px 0 10px;line-height:1.35;\">Kaynak<\/h4>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">Kaynak \u00b7 Hastelloy B-3<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">\u00d6nerilen prosesler<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>TIG\/GTAW, MIG\/GMAW, \u00f6rt\u00fcl\u00fc elektrot\/SMAW<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>\u00d6NER\u0130LMEYEN<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>Oksi-asetilen ve TOZALTI kayna\u011f\u0131 \u00f6nerilmez.<\/b> <b>Dikkat:<\/b> en az bir da\u011f\u0131t\u0131mc\u0131 sayfas\u0131 bu c\u00fcmleyi <b>tam tersine \u00e7evirmi\u015f<\/b> h\u00e2lde yay\u0131ml\u0131yor \u2014 imalat\u00e7\u0131 ona g\u00f6re davran\u0131rsa ger\u00e7ekten tehlikeli bir hatad\u0131r<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">\u00c7\u0131plak tel \u00b7 elektrot<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>ERNiMo-10<\/b> (A5.14, UNS N10675) \u00b7 <b>ENiMo-10<\/b> (A5.11) \u00b7 DIN 2.4695 \/ 2.4696<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>ERNiMo-7 KULLANMAYIN<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>O, B-2 dolgusudur.<\/b> Daha d\u00fc\u015f\u00fck Fe, Cr ve Mn ta\u015f\u0131r ve <b>B-2&#8217;nin d\u00fczenlenme davran\u0131\u015f\u0131n\u0131 do\u011frudan B-3 birle\u015fiminin kaynak metaline koyar<\/b> \u2014 tam da B-3 sat\u0131n alarak ka\u00e7\u0131nd\u0131\u011f\u0131n\u0131z kusur<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">\u00d6n tav<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>Gerekli de\u011fildir.<\/b> Kaynak \u00f6ncesi ve sonras\u0131 i\u015flem &#8220;genellikle gereksiz&#8221;<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Pasolar aras\u0131 s\u0131cakl\u0131k<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>D\u00fc\u015f\u00fck tutun.<\/b> <b>Yay\u0131mlanm\u0131\u015f say\u0131sal bir tavan bulunamad\u0131 \u2014 bir rakam yay\u0131mlamay\u0131n.<\/b> Ni-Mo ala\u015f\u0131mlar\u0131nda pratik, m\u00fcteahhit prosed\u00fcr\u00fcne g\u00f6re olabilecek en d\u00fc\u015f\u00fck de\u011ferde \u00e7al\u0131\u015fmakt\u0131r<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Is\u0131 girdisi<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">&#8220;<b>A\u015f\u0131r\u0131 \u0131s\u0131 girdisinden ka\u00e7\u0131nmak i\u00e7in \u00f6zel \u00f6nlem al\u0131nmal\u0131d\u0131r<\/b>&#8221; \u00b7 <b>say\u0131sal bir kJ\/mm limiti yay\u0131mlanmam\u0131\u015ft\u0131r<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">PWHT<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>Normalde gerekli de\u011fildir.<\/b> \u2264%0,010 C duyarl\u0131la\u015ft\u0131r\u0131c\u0131 karb\u00fcr \u00e7\u00f6kelmesi b\u0131rakmaz ve B-3&#8217;\u00fcn d\u00fczenlenme kineti\u011fi normal bir kaynak \u00e7evrimini kald\u0131racak kadar yava\u015ft\u0131r. Kaynak sonras\u0131 \u00e7\u00f6zelti tav\u0131 <b>a\u011f\u0131r servise<\/b> veya <b>\u00f6ncesinde a\u011f\u0131r so\u011fuk i\u015f yap\u0131lm\u0131\u015f<\/b> par\u00e7alara ayr\u0131lm\u0131\u015ft\u0131r<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p style=\"margin:18px 0 6px;font-size:15px;font-weight:700;color:#12303f;line-height:1.5;\">Ger\u00e7ekte ne ters gidiyor<\/p>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>1. So\u011fuk i\u015flenmi\u015f malzemenin \u00fczerine kaynak yapmak.<\/b> En \u00e7ok an\u0131lan ar\u0131za bi\u00e7imi. So\u011fuk i\u015f ~%7&#8217;yi a\u015fm\u0131\u015f ve tavla giderilmemi\u015fse B-3 &#8220;<b>sonraki imalat\/kaynak s\u0131ras\u0131nda kaynak b\u00f6lgesinde \u00e7atlamaya \u00e7ok yatk\u0131nd\u0131r<\/b>&#8220;. <b>So\u011fuk \u015fekillendirilmi\u015f bombeleri, b\u00fck\u00fclm\u00fc\u015f borular\u0131, haddelenmi\u015f g\u00f6vdeleri ve mandrellenmi\u015f boru u\u00e7lar\u0131n\u0131 kaynaktan \u00d6NCE \u00e7\u00f6zelti tav\u0131na al\u0131n.<\/b><br \/><b>2. \u00c7ok pasolu kaynakta \u0131s\u0131 girdisinin birikmesi.<\/b> E\u011frinin burnu 650 \u00b0C&#8217;de ve kulu\u00e7ka birka\u00e7 saat; yani <b>tek bir kaynak zarar vermez<\/b> \u2014 ama s\u0131cak tutulan a\u011f\u0131r \u00e7ok pasolu bir birle\u015fim, art\u0131 yava\u015f bir gerilim giderme, art\u0131 bir s\u0131cak \u015fekillendirme yeniden \u0131s\u0131tmas\u0131 <b>birikir<\/b>. <b>Yaln\u0131zca tepe s\u0131cakl\u0131\u011f\u0131n\u0131 de\u011fil, 500\u2013900 \u00b0C&#8217;de ge\u00e7en k\u00fcm\u00fclatif s\u00fcreyi izleyin.<\/b><br \/><b>3. S\u00fclf\u00fcrik asitte kaynak metali cezas\u0131.<\/b> \u00dcreticinin kendi kaynak\/ana metal verisi, 93 \u00b0C: <b>%50 H\u2082SO\u2084&#8217;te kaynak 0,13 mm\/y\u0131l, ana metal 0,04 mm\/y\u0131l \u2014 3,3 kat ceza<\/b>; %70 H\u2082SO\u2084&#8217;te 0,03&#8217;e kar\u015f\u0131 0,01. Buna kar\u015f\u0131l\u0131k <b>HCl&#8217;de kaynak ve ana metal ayn\u0131d\u0131r<\/b> (%5 HCl: ikisi de 0,30 mm\/y\u0131l; %10 HCl: ikisi de 0,29). Yani <b>HCl&#8217;de kaynak zay\u0131f nokta de\u011fildir; s\u00fclf\u00fcrik asitte \u00f6yledir<\/b> \u2014 ger\u00e7ekten yararl\u0131 bir ayr\u0131m ve neredeyse hi\u00e7 kimse yay\u0131mlam\u0131yor.<br \/><b>4. Temizlik.<\/b> Par\u00e7alar kaynaktan \u00f6nce &#8220;gerilimsiz, temiz ve kirleticiden ar\u0131nm\u0131\u015f&#8221; olmal\u0131d\u0131r. <b>K\u00fck\u00fcrt, kur\u015fun, \u00e7inko ve bak\u0131r bula\u015fmas\u0131 t\u00fcm y\u00fcksek nikelli ala\u015f\u0131mlarda s\u0131cak \u00e7atlama yapar.<\/b><\/p>\n<h4 id=\"dm-b8\" style=\"font-size:19px;font-weight:700;color:#12303f;margin:30px 0 10px;line-height:1.35;\">Tala\u015fl\u0131 \u0130malat<\/h4>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>A\u00e7\u0131k\u00e7a belirtilmesi gereken \u00e7ekince:<\/b> \u00fcretici, <b>B-3&#8217;e \u00f6zg\u00fc<\/b> bir h\u0131z\/ilerleme tablosu de\u011fil, <b>korozyona dayan\u0131kl\u0131 ala\u015f\u0131m ailesi<\/b> i\u00e7in parametre yay\u0131mlar. A\u015fa\u011f\u0131dakileri &#8220;<b>\u00e7\u00f6zelti tavl\u0131 korozyona dayan\u0131kl\u0131 ala\u015f\u0131mlar (B-3 d\u00e2hil) i\u00e7in ba\u015flang\u0131\u00e7 parametreleri<\/b>&#8221; olarak yay\u0131mlay\u0131n, B-3 verisi olarak de\u011fil.<\/p>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">Ba\u015flang\u0131\u00e7 Parametreleri (aile rehberi)<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Tornalama \u00b7 kaba<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">Karb\u00fcr <b>C-2\/C-3, negatif tala\u015f a\u00e7\u0131s\u0131<\/b> \u00b7 <b>27 m\/dak (90 sfm)<\/b> \u00b7 ilerleme <b>0,25 mm\/dev<\/b> \u00b7 tala\u015f derinli\u011fi &lt;3,8 mm<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Tornalama \u00b7 fini\u015f<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">Karb\u00fcr, <b>pozitif tala\u015f a\u00e7\u0131s\u0131<\/b>, 0,8 mm u\u00e7 rady\u00fcs\u00fc \u00b7 <b>29\u201334 m\/dak<\/b> \u00b7 ilerleme <b>0,13\u20130,18 mm\/dev<\/b> \u00b7 derinlik 1,0 mm<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Delme<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">HSS M-33\/M-40\/T-15 <b>3\u20134,6 m\/dak<\/b> \u00b7 karb\u00fcr C-2 <b>15 m\/dak<\/b> \u00b7 ilerleme 0,05 mm (\u23006) \u2192 0,18 mm (\u230025)<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Parmak freze<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">HSS M-40\/T-15 <b>6\u20137,6 m\/dak<\/b>, di\u015f ba\u015f\u0131na 0,05\u20130,10 mm \u00b7 karb\u00fcr C-2 <b>\u00fcretici &#8220;marjinal ba\u015far\u0131m&#8221; diyor<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Raybalama \u00b7 k\u0131lavuz \u00e7ekme<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">Rayba <b>3\u20134,6 m\/dak<\/b> \u00b7 k\u0131lavuz <b>7 sfm<\/b>, &#8220;<b>m\u00fcmk\u00fcn olan en iyi k\u0131lavuz \u00e7ekme bile\u015fi\u011fini kullan\u0131n; s\u00fclfo-klorlu ya\u011f bazl\u0131 tercih edilir<\/b>&#8220;<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Y\u00f6neten kurallar<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">Ala\u015f\u0131m ostenitik paslanmazdan daha h\u0131zl\u0131 pekle\u015fir: <b>rijit ba\u011flama, pozitif ilerleme, asla bekletmeyin ve asla s\u00fcrtmeyin<\/b> \u2014 duran bir ilerleme y\u00fczeyi parlat\u0131r ve bir sonraki paso pekle\u015fmi\u015f bir kabu\u011fu kesmek zorunda kal\u0131r. <b>S\u00fclfo-klorlu k\u0131lavuz bile\u015fi\u011fi her t\u00fcrl\u00fc \u0131s\u0131l i\u015flem veya kaynaktan \u00f6nce tamamen giderilmelidir<\/b> \u2014 kal\u0131nt\u0131 k\u00fck\u00fcrt s\u0131cak \u00e7atlama yapar<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<h4 id=\"dm-b9\" style=\"font-size:19px;font-weight:700;color:#12303f;margin:30px 0 10px;line-height:1.35;\">Korozyon \u2014 Davran\u0131\u015f Neden \u0130kili<\/h4>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>B-3&#8217;te ~%1,5 krom vard\u0131r. Krom oksit pasif filmi olu\u015fturmaz.<\/b> Asitlerdeki korozyon direnci, molibdenin <b>hidrojen a\u015f\u0131r\u0131 gerilimini y\u00fckseltip indirgeyici katodik reaksiyonu bast\u0131rmas\u0131ndan<\/b> gelir. Sonu\u00e7: <b>mevcut tek katodik reaksiyon hidrojen \u00e7\u0131k\u0131\u015f\u0131 oldu\u011funda \u00fcst\u00fcn; daha g\u00fc\u00e7l\u00fc bir y\u00fckseltgen bulundu\u011fu anda \u00e7ok k\u00f6t\u00fc.<\/b> A\u015fa\u011f\u0131daki her sat\u0131r bu tek c\u00fcmleden \u00e7\u0131kar.<\/p>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">Hidroklorik Asit \u2014 Amiral G\u00f6rev (mm\/y\u0131l, reaktif safl\u0131kta)<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">%1 HCl<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">38 \u00b0C <b>0,07<\/b> \u00b7 52 \u00b0C 0,11 \u00b7 66 \u00b0C 0,18 \u00b7 93 \u00b0C 0,21 \u00b7 kaynama <b>0,01<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">%2 HCl<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">0,10 \u00b7 0,16 \u00b7 0,21 \u00b7 0,26 \u00b7 0,04<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">%5 HCl<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">0,11 \u00b7 0,19 \u00b7 0,25 \u00b7 <b>0,30<\/b> \u00b7 0,08<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">%10 HCl<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">0,13 \u00b7 0,20 \u00b7 0,24 \u00b7 0,29 \u00b7 0,13<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">%15 HCl<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">0,10 \u00b7 0,18 \u00b7 0,23 \u00b7 0,28 \u00b7 0,21<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">%20 HCl<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">0,10 \u00b7 0,15 \u00b7 0,21 \u00b7 <b>0,30<\/b> \u00b7 0,29<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>\u00dcreticinin korozyon rehberi<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">&#8220;<b>Saf hidroklorik aside en y\u00fcksek dirence sahip ala\u015f\u0131mlar, molibden i\u00e7erikleri %30&#8217;a yak\u0131n olan nikel-molibden ailesindekilerdir.<\/b>&#8221; Not: kaynama sat\u0131r\u0131 seyreltik deri\u015fimlerde 93 \u00b0C sat\u0131r\u0131ndan <b>daha d\u00fc\u015f\u00fckt\u00fcr<\/b> \u2014 bu ger\u00e7ektir ve HCl&#8217;nin \u00e7\u00f6zeltiden u\u00e7mas\u0131n\u0131n etkisidir<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">S\u00fclf\u00fcrik ve Di\u011fer Asitler (mm\/y\u0131l)<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">H\u2082SO\u2084 %10<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">38 \u00b0C 0,04 \u00b7 66 \u00b0C 0,11 \u00b7 93 \u00b0C 0,11 \u00b7 kaynama 0,01<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">H\u2082SO\u2084 %30<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">38 \u00b0C 0,02 \u00b7 66 \u00b0C 0,06 \u00b7 93 \u00b0C 0,09 \u00b7 kaynama 0,02<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">H\u2082SO\u2084 %50<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">66 \u00b0C 0,03 \u00b7 93 \u00b0C <b>0,04<\/b> \u00b7 kaynama 0,03<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">H\u2082SO\u2084 %70<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">93 \u00b0C 0,01 \u00b7 kaynama <b>0,15<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>H\u2082SO\u2084 %80<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">93 \u00b0C 0,01 \u00b7 <b>177 \u00b0C 0,44<\/b> \u00b7 <b>kaynama 4,76<\/b> \u2014 iki mertebe s\u0131\u00e7rama<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">H\u2082SO\u2084 %90\u201396<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">93 \u00b0C 0,02<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Hidrobromik asit<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">%2,5: 38 \u00b0C 0,07 \/ 66 \u00b0C 0,26 \/ 93 \u00b0C 0,24 \/ kaynama 0,02 \u00b7 %30: 0,10 \/ 0,20 \/ 0,29 \/ <b>0,29<\/b> \u00b7 %40: 0,06 \/ 0,16 \/ 0,25 \/ <b>0,43<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\">Fosforik asit, kaynar<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">%10 0,07 \u00b7 %30 0,07 \u00b7 %50 0,09 \u00b7 %60 0,14 \u00b7 <b>%70 0,21<\/b> \u00b7 %80 0,04 \u00b7 %85 0,10<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Organik asitler, kaynar<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\"><b>Asetik asit %10\u201399: 0,01\u20130,02 mm\/y\u0131l<\/b> \u00b7 <b>formik asit %10\u201389: 0,01\u20130,02 mm\/y\u0131l<\/b> \u2014 fiilen inert<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Gerilmeli korozyon (ASTM G36)<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">Kaynar %45 MgCl\u2082: <b>B-3 \u2014 1.008 saatte \u00e7atlama yok<\/b>. Ayn\u0131 tabloda ba\u011flam: <b>316L 2 saatte<\/b>, 254 SMO 24 saatte \u00e7atlad\u0131; ala\u015f\u0131m 625 ve C-276 de 1.008 saat dayand\u0131. Flor\u00fcrl\u00fc ortamlara da diren\u00e7li<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<div style=\"border:1px solid #d7dfe4;background:#ffffff;margin:24px 0 18px;position:relative;overflow:hidden;\">\n<div style=\"background:#DD3333;color:#ffffff;font-size:13px;font-weight:700;letter-spacing:.04em;text-transform:uppercase;padding:10px 12px;line-height:1.35;\">NEREDE BA\u015eARISIZ \u2014 Bunu En Az \u0130yi Haber Kadar Belirgin Yay\u0131mlay\u0131n<\/div>\n<p><span aria-hidden=\"true\" data-dmwm=\"1\" style=\"position:absolute;top:50%;left:50%;transform:translate(-50%,-50%) rotate(-18deg);font-size:72px;font-weight:800;letter-spacing:.12em;color:#12303f;opacity:.05;white-space:nowrap;pointer-events:none;user-select:none;z-index:3;\">DEFENCE METAL<\/span><\/p>\n<table style=\"border-collapse:collapse;width:100%;font-size:15px;line-height:1.5;\">\n<tbody>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Nitrik asit<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">\u00dcreticinin korozyon rehberi aynen: &#8220;<b>krom i\u00e7eri\u011fi yaln\u0131zca a\u011f\u0131rl\u0131k\u00e7a %1,5 olan B-3 ala\u015f\u0131m\u0131 nitrik asitte h\u0131zla korozyona u\u011frar<\/b>&#8220;. <b>Nitrik servis, kar\u0131\u015f\u0131k asit veya nitrik i\u00e7eren hi\u00e7bir asitleme\/pasifle\u015ftirme hatt\u0131 i\u00e7in B-3 teklif etmeyin<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Ferrik (Fe\u00b3\u207a) ve kuprik (Cu\u00b2\u207a) iyonlar\u0131 \u2014 klasik saha ar\u0131zas\u0131<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>&#8220;B-3 ala\u015f\u0131m\u0131 ferrik veya kuprik tuzlar\u0131n varl\u0131\u011f\u0131nda kullan\u0131lmas\u0131 \u00d6NER\u0130LMEZ; bu tuzlar h\u0131zl\u0131 korozyon ar\u0131zas\u0131na yol a\u00e7abilir.&#8221;<\/b> Be\u015f ba\u011f\u0131ms\u0131z yay\u0131nc\u0131 ayn\u0131 c\u00fcmleyi ta\u015f\u0131yor. <b>Say\u0131:<\/b> <b>%20 HCl, temiz, 93 \u00b0C \u2192 0,30 mm\/y\u0131l<\/b> \u00b7 <b>%20 HCl + 50 ppm Fe\u00b3\u207a, 93 \u00b0C \u2192 2,0 mm\/y\u0131l<\/b>. <b>Milyonda elli ferrik iyon korozyon h\u0131z\u0131n\u0131 kabaca 6,6 KATINA \u00e7\u0131kar\u0131r.<\/b> 50 ppm hi\u00e7bir \u015feydir: HCl bir karbon \u00e7eli\u011fi pompaya, yumu\u015fak \u00e7elik bir fittinge, pasl\u0131 bir varile, \u00e7elik bir vana i\u00e7 par\u00e7as\u0131na veya yukar\u0131 ak\u0131\u015ftaki karbon \u00e7eli\u011fi bir hatta temas etti\u011finde elde edece\u011finiz \u015feydir. <b>Bu bir laboratuvar \u00e7ekincesi de\u011fil \u2014 B ala\u015f\u0131mlar\u0131n\u0131n serviste ar\u0131zalanmas\u0131n\u0131n en yayg\u0131n tek sebebidir<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Havaland\u0131r\u0131lm\u0131\u015f \/ oksijenli asit, \u00e7\u00f6z\u00fcnm\u00fc\u015f oksijen, \u0131slak klor<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">H\u207a\/H\u2082 indirgenmesinden daha g\u00fc\u00e7l\u00fc bir katodik reaksiyon sa\u011flayan her y\u00fckseltgen sald\u0131r\u0131r. <b>Y\u00fckseltgen klor\u00fcrler, hipoklorit ve \u0131slak Cl\u2082 kapsam d\u0131\u015f\u0131d\u0131r<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>Kaynar s\u00fclf\u00fcrik asit ~%80 \u00fczeri<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\"><b>%80 a\u011f\u0131rl\u0131kta kaynamada 4,76 mm\/y\u0131l<\/b> ve %80 \/ 177 \u00b0C&#8217;de 0,44 mm\/y\u0131l \u2014 %70 alt\u0131ndaki her yerde 0,01\u20130,05 mm\/y\u0131l iken. <i>(Bu 4,76 rakam\u0131n\u0131n %80 mi %96 m\u0131 oldu\u011funa dair iki okuma var; g\u00fcvenli m\u00fchendislik ifadesi: &#8220;<b>kaynar s\u00fclf\u00fcrik asitte ~%80 \u00fczerinde korozyon iki mertebe h\u0131zlan\u0131r<\/b>&#8220;)<\/i><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\">Y\u00fckseltgenli s\u00fclf\u00fcrik asit<\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">&#8220;S\u00fclf\u00fcrik asitte y\u00fckseltgen t\u00fcrlerin varl\u0131\u011f\u0131 nikel-molibden ala\u015f\u0131mlar\u0131n\u0131 olumsuz etkiler&#8221;<\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;\"><b>C-276&#8217;n\u0131n yerine ge\u00e7mez<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;\">C-276 ~%16 Cr&#8217;li Ni-Cr-Mo-W&#8217;dur: y\u00fckseltgen ko\u015fullara ve kar\u0131\u015f\u0131k ortamlara dayan\u0131r, ama <b>saf indirgeyici HCl&#8217;de B-3 onu yener<\/b>. Farkl\u0131 sorunlar\u0131 \u00e7\u00f6zerler. <b>Tesiste hem indirgeyici asit hem herhangi bir y\u00fckseltgen varsa cevap bir Ni-Cr-Mo ala\u015f\u0131m\u0131d\u0131r<\/b> (<a href=\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-c-276\/\">C-276<\/a>, <a href=\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-c-22\/\">C-22<\/a>), <b>B-3 de\u011fil<\/b><\/td>\n<\/tr>\n<tr>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;font-weight:700;color:#12303f;width:42%;background:#F7FAFB;\"><b>Standart \u00e7ekince<\/b><\/td>\n<td style=\"padding:7px 12px;border-top:1px solid #eceff1;background:#F7FAFB;\">&#8220;T\u00fcm korozyon verileri reaktif safl\u0131kta asit laboratuvar testlerinden t\u00fcretilmi\u015ftir; saha do\u011frulamas\u0131 \u00f6nerilir.&#8221; <b>Bu c\u00fcmlenin bir s\u00fcr\u00fcm\u00fcn\u00fc sayfaya koyun<\/b> \u2014 ayn\u0131 zamanda ticari koruman\u0131zd\u0131r<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<h4 id=\"dm-b10\" style=\"font-size:19px;font-weight:700;color:#12303f;margin:30px 0 10px;line-height:1.35;\">S\u0131k Sorulan Sorular<\/h4>\n<p style=\"margin:18px 0 6px;font-size:15px;font-weight:700;color:#12303f;line-height:1.5;\">Zaten B-2 kullan\u0131yoruz. B-3&#8217;e para vermeye de\u011fer mi, yoksa bu sadece yeni bir par\u00e7a numaras\u0131 m\u0131?<\/p>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>De\u011fer, ve gerek\u00e7e dar ve \u00f6zg\u00fcld\u00fcr: serviste korozyon direnci de\u011fil, imalat ve ar\u0131za ko\u015fullar\u0131ndaki \u0131s\u0131l kararl\u0131l\u0131k.<\/b> Temiz, kirlenmemi\u015f hidroklorik asitte iki ala\u015f\u0131m \u00e7ok benzer davran\u0131r; hik\u00e2ye bundan ibaret olsayd\u0131 B-2 almaya devam etmeniz gerekirdi.<br \/>Farkl\u0131 olan \u015fey, metalin kabaca <b>500 ile 900 \u00b0C<\/b> aras\u0131nda ba\u015f\u0131na gelenlerdir. Karbonu al\u0131nm\u0131\u015f olan B-2, gevrek <b>Ni\u2084Mo \u03b2 faz\u0131na \u00e7ok h\u0131zl\u0131 d\u00fczenlenir<\/b> \u2014 \u00fcretici <b>700 \u00b0C&#8217;de yar\u0131m il\u00e2 bir saatte on Rockwell-A puan\u0131ndan fazla sertle\u015fme<\/b> \u00f6l\u00e7m\u00fc\u015ft\u00fcr. Bu, bir kaynak \u0131s\u0131 tesiri alt\u0131ndaki b\u00f6lgede, yava\u015f so\u011fuyan a\u011f\u0131r bir kesitin merkezinde, s\u0131cak \u015fekillendirmede ve herhangi bir proses a\u015f\u0131m\u0131nda olur. Sonu\u00e7 tane s\u0131n\u0131r\u0131 gevrekle\u015fmesi ve taneler aras\u0131 bir korozyon yoludur. \u00dcreticinin kendi yan yana testi: <b>700 \u00b0C maruziyetinden sonra kaynar %60 s\u00fclf\u00fcrikte B-2 \u00fc\u00e7 saatte taneler aras\u0131 \u00e7atlarken B-3 yirmi d\u00f6rt saatte h\u00e2l\u00e2 \u00e7atlamam\u0131\u015ft\u0131.<\/b><br \/>B-3 bunu, B-2&#8217;nin \u00e7\u0131kard\u0131\u011f\u0131n\u0131 <b>bilin\u00e7le geri ekleyerek<\/b> ba\u015far\u0131r \u2014 asgari %1,0&#8217;er krom ve demir, %3&#8217;e kadar manganez ve al\u00fcminyum \u2014 ve reaksiyonu \u00e7ok daha yava\u015f olan <b>Ni\u2083Mo<\/b>&#8216;ya sapt\u0131r\u0131r. Patentin pratik sonucu a\u00e7\u0131kt\u0131r: <b>\u0131s\u0131tma ve so\u011futma s\u00fcreleri B-2 i\u00e7in \u00f6nerilenlerden yakla\u015f\u0131k on kat daha yava\u015f olabilir.<\/b><br \/><b>Yani:<\/b> bir kaba kaynaklanacak levha al\u0131yorsan\u0131z, s\u0131cak \u015fekillendirecekseniz, a\u011f\u0131r kesit kaynaklayacaksan\u0131z veya o s\u0131cakl\u0131k band\u0131na proses a\u015f\u0131mlar\u0131n\u0131z varsa, B-3 <b>ger\u00e7ek ve belgelenmi\u015f bir ar\u0131za bi\u00e7imini ortadan kald\u0131r\u0131r<\/b>. \u0130nce, zaten tavl\u0131, kaynaklanmayacak sac al\u0131yor ve so\u011fuk asitte kullanacaksan\u0131z avantaj daha k\u00fc\u00e7\u00fckt\u00fcr. <b>Ala\u015f\u0131m\u0131 de\u011fil, riski fiyatland\u0131r\u0131n.<\/b><\/p>\n<p style=\"margin:18px 0 6px;font-size:15px;font-weight:700;color:#12303f;line-height:1.5;\">Sayfan\u0131z B-3&#8217;\u00fcn her deri\u015fim ve s\u0131cakl\u0131kta HCl&#8217;ye dayand\u0131\u011f\u0131n\u0131 yaz\u0131yor. HCl hatt\u0131m\u0131z\u0131n yukar\u0131 ak\u0131\u015f\u0131 karbon \u00e7eli\u011fi. Sorun olur mu?<\/p>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>Olur \u2014 ve en s\u0131k g\u00f6rd\u00fc\u011f\u00fcm\u00fcz ar\u0131za budur.<\/b> O &#8220;her deri\u015fim ve s\u0131cakl\u0131k&#8221; iddias\u0131 yaln\u0131zca <b>saf, havas\u0131 al\u0131nm\u0131\u015f, kirlenmemi\u015f<\/b> hidroklorik asit i\u00e7in do\u011frudur ve karbon \u00e7eli\u011fi yukar\u0131 ak\u0131\u015f\u0131n\u0131z b\u00f6yle bir asidinizin <b>olmad\u0131\u011f\u0131n\u0131<\/b> garanti eder.<br \/>B-3&#8217;te yakla\u015f\u0131k <b>%1,5 krom<\/b> vard\u0131r. <b>Pasif oksit filmi yoktur.<\/b> Direnci, molibdenin hidrojen \u00e7\u0131k\u0131\u015f reaksiyonunu bast\u0131rmas\u0131ndan gelir \u2014 ki bu, mevcut tek katodik reaksiyon hidrojen \u00e7\u0131k\u0131\u015f\u0131 oldu\u011fu s\u00fcrece m\u00fckemmel \u00e7al\u0131\u015f\u0131r. Daha g\u00fc\u00e7l\u00fc bir y\u00fckseltgen girdi\u011fi anda o koruma <b>basit\u00e7e yoktur<\/b>.<br \/>Ferrik iyon tam olarak o y\u00fckseltgendir ve HCl i\u00e7indeki karbon \u00e7eli\u011fi onu <b>s\u00fcrekli \u00fcretir<\/b>. Yay\u0131mlanm\u0131\u015f say\u0131: <b>93 \u00b0C&#8217;de %20 HCl, B-3&#8217;\u00fc 0,30 mm\/y\u0131l<\/b> korozyona u\u011frat\u0131r. Ayn\u0131 asit <b>50 ppm ferrik iyonla 2,0 mm\/y\u0131l<\/b> \u2014 yakla\u015f\u0131k <b>6,6 kat h\u0131zl\u0131<\/b>. Elli ppm bir eser miktard\u0131r: tek bir pasl\u0131 flan\u015f, tek bir \u00e7elik vana i\u00e7 par\u00e7as\u0131, tek bir karbon \u00e7eli\u011fi pompa g\u00f6vdesi bunu \u00fcretir. Bak\u0131r i\u00e7eren herhangi bir bile\u015fenden gelen kuprik iyon ayn\u0131 \u015feyi yapar. Hem \u00fcretici hem her ciddi Avrupa fabrika sayfas\u0131 &#8220;<b>ferrik veya kuprik tuzlar\u0131n varl\u0131\u011f\u0131nda \u00f6nerilmez<\/b>&#8221; c\u00fcmlesini ta\u015f\u0131r.<br \/><b>Pratikte \u00fc\u00e7 se\u00e7ene\u011finiz var.<\/b> Asidin temiz kalmas\u0131 i\u00e7in yukar\u0131 ak\u0131\u015ftaki karbon \u00e7eli\u011fini de\u011fi\u015ftirin. Ak\u0131\u015fa <b>ferrik\/kuprik analizi tak\u0131n ve ger\u00e7ekten izleyin<\/b> \u2014 \u00fc\u00e7 ayda bir numune de\u011fil, alarm kurun. Ya da y\u00fckseltgene dayanan bir nikel-krom-molibden ala\u015f\u0131m\u0131 se\u00e7in (<a href=\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-c-276\/\">C-276<\/a> veya <a href=\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-c-22\/\">C-22<\/a>), saf HCl&#8217;deki bir miktar ba\u015far\u0131m\u0131 feda ederek. <b>Bu hat i\u00e7in B-3 teklif ederiz, ama ferrik iyon k\u0131s\u0131t\u0131n\u0131 sipari\u015f teyidine yazar\u0131z<\/b>: de\u011fi\u015fken ala\u015f\u0131m de\u011fil, kirlenmedir.<\/p>\n<p style=\"margin:18px 0 6px;font-size:15px;font-weight:700;color:#12303f;line-height:1.5;\">M\u00fc\u015fterinin \u015fartnamesi B-3, ASME B\u00f6l\u00fcm VIII, 450 \u00b0C servis diyor. Verebilir miyiz?<\/p>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>O tasar\u0131m s\u0131cakl\u0131\u011f\u0131nda bas\u0131n\u00e7 ta\u015f\u0131yan malzeme olarak hay\u0131r \u2014 ve sebep metalurjik de\u011fil, bir kod limitidir. Bu ikisi farkl\u0131 \u015feylerdir ve hangisine \u00e7arpt\u0131\u011f\u0131n\u0131z \u00f6nemlidir.<\/b><br \/><b>Metalurjik olarak<\/b> B-3 450 \u00b0C&#8217;de gayet servis edilebilirdir: \u00fcretici <b>649 \u00b0C&#8217;ye kadar tipik \u00e7ekme verisi<\/b> ve <b>540 \u00b0C&#8217;de 16.000 saat sonra uzaman\u0131n h\u00e2l\u00e2 %43,7<\/b> oldu\u011funu g\u00f6steren maruziyet verisi yay\u0131mlar. Ala\u015f\u0131m 450 \u00b0C&#8217;de zorda de\u011fildir.<br \/><b>Sorun kod kapsam\u0131d\u0131r.<\/b> <b>ASME B\u00f6l\u00fcm VIII Div. 1 B-3&#8217;\u00fc yaln\u0131zca 427 \u00b0C (800 \u00b0F)&#8217;ye kabul eder.<\/b> \u00dcst\u00fcnde emniyet gerilmesi yoktur. <b>ASME B31.3<\/b> ayn\u0131 427 \u00b0C&#8217;de durur. M\u00fc\u015fteriniz Avrupa yolundaysa <b>VdT\u00dcV Malzeme Sayfas\u0131 517 daha da d\u00fc\u015f\u00fck, 400 \u00b0C&#8217;de<\/b> durur. Ta\u015f\u0131ma tanklar\u0131 i\u00e7in <b>B\u00f6l\u00fcm XII 343 \u00b0C<\/b>&#8216;de durur. Yani 450 \u00b0C&#8217;de, hangi kodda olursan\u0131z olun, <b>tasar\u0131m yapacak bir emniyet gerilmesi yoktur<\/b>.<br \/><b>\u0130nsanlar\u0131 yakalayan \u00fc\u00e7 kapsam ger\u00e7e\u011fi daha:<\/b> B-3 <b>B\u00f6l\u00fcm VIII Division 2&#8217;de kabul edilmez<\/b>, <b>B\u00f6l\u00fcm I&#8217;de kabul edilmez<\/b> ve <b>B31.1&#8217;de kabul edilmez<\/b>. Kap bir Div. 2 tasar\u0131m\u0131ysa, B-3 bir kod davas\u0131 olmadan bas\u0131n\u00e7 s\u0131n\u0131r\u0131 olamaz.<br \/><b>Ger\u00e7ek\u00e7i cevaplar:<\/b> proses ger\u00e7ekten izin veriyorsa tasar\u0131m s\u0131cakl\u0131\u011f\u0131n\u0131 427 \u00b0C&#8217;ye d\u00fc\u015f\u00fcrt\u00fcn; yukar\u0131da kod kapsam\u0131 olan bir Ni-Cr-Mo ala\u015f\u0131m\u0131na ge\u00e7in (<a href=\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-c-276\/\">C-276<\/a> veya <a href=\"https:\/\/www.defencemetal.com\/index.php\/inconel-625\/\">ala\u015f\u0131m 625<\/a>); ya da B-3&#8217;\u00fc kod onayl\u0131 bir ta\u015f\u0131y\u0131c\u0131 malzeme \u00fczerinde <b>bas\u0131n\u00e7 ta\u015f\u0131mayan astar veya i\u00e7 par\u00e7a<\/b> olarak kullan\u0131n. <b>Yapmaman\u0131z gereken \u015fey, bir mekanik \u00f6zellik tablosundan &#8220;B-3 650 \u00b0C&#8217;ye kadar iyidir&#8221; al\u0131nt\u0131lay\u0131p bunun bir tasar\u0131m s\u0131cakl\u0131\u011f\u0131na d\u00f6n\u00fc\u015fmesine izin vermektir. O bir kabiliyet rakam\u0131d\u0131r ve kod onu kabul etmez.<\/b><\/p>\n<p style=\"margin:18px 0 6px;font-size:15px;font-weight:700;color:#12303f;line-height:1.5;\">Veri sayfalar\u0131nda s\u0131k rastlanan hatalar \u2014 sipari\u015f vermeden \u00f6nce kontrol edin<\/p>\n<p style=\"margin:0 0 12px;font-size:15px;line-height:1.75;\"><b>1. &#8220;AMS 5891&#8221; B-3 levha \u015fartnamesi diye an\u0131l\u0131yor \u2014 YANLI\u015e.<\/b> AMS 5891 <b>60Ni-22Cr-2Mo-14W<\/b> bir ala\u015f\u0131m\u0131n <b>\u00e7ubuk\/d\u00f6vme\/halka<\/b> \u015fartnamesidir, bamba\u015fka bir malzemedir. <b>B-3 i\u00e7in AMS \u015fartnamesi yoktur.<\/b><br \/><b>2. &#8220;AMS 5396&#8221; B-3 e\u015fde\u011feri diye an\u0131l\u0131yor \u2014 YANLI\u015e.<\/b> O, <b>65Ni-28Mo-5,5Fe-0,4V (N-12MV) hassas d\u00f6k\u00fcm<\/b> \u015fartnamesidir \u2014 yani <b>d\u00f6k\u00fcm ala\u015f\u0131m-B<\/b> bile\u015fimi; B-3&#8217;\u00fcn \u00f6zellikle d\u0131\u015flad\u0131\u011f\u0131 %5,5 demir ve %0,4 vanadyum ile.<br \/><b>3. ERNiMo-7 \/ ENiMo-7 B-3 dolgusu diye an\u0131l\u0131yor \u2014 YANLI\u015e, o B-2 dolgusudur.<\/b> Do\u011frusu <b>ERNiMo-10 \/ ENiMo-10, ikisi de UNS N10675<\/b>.<br \/><b>4. ASME P numaras\u0131 112 diye veriliyor \u2014 YANLI\u015e.<\/b> B-3 <b>P-No. 44 \/ F-No. 44<\/b>&#8216;t\u00fcr.<br \/><b>5. W.Nr. kar\u0131\u015f\u0131kl\u0131\u011f\u0131:<\/b> <b>2.4600 = B-3<\/b>, <b>2.4617 = B-2<\/b>, <b>2.4800 = ala\u015f\u0131m B<\/b>. Ayr\u0131ca <b>2.4695 ve 2.4696 DOLGU metali numaralar\u0131d\u0131r<\/b>, ana metal kalitesi de\u011fil.<br \/><b>6. EN ad\u0131:<\/b> \u00fcretici ve iki Alman fabrikas\u0131 <b>NiMo29Cr<\/b> yazar \u2014 \u00e7o\u011funluk ve fabrika duru\u015fu budur. <b>NiMo30Cr asl\u0131nda do\u011frudur ama KAYNAK TEL\u0130 (2.4695) i\u00e7in<\/b>; hatan\u0131n kayna\u011f\u0131 b\u00fcy\u00fck olas\u0131l\u0131kla budur.<br \/><b>7. &#8220;Azami \u00e7al\u0131\u015fma s\u0131cakl\u0131\u011f\u0131 400 \u00b0C&#8221; bir malzeme \u00f6zelli\u011fi gibi yay\u0131mlan\u0131yor.<\/b> 400 \u00b0C <b>VdT\u00dcV 517 kod tavan\u0131d\u0131r<\/b>; ASME VIII Div. 1 <b>427 \u00b0C<\/b> verir; \u00fcretici <b>649 \u00b0C<\/b>&#8216;ye kadar mekanik veri ve <b>540 \u00b0C<\/b>&#8216;de uzun s\u00fcreli kararl\u0131l\u0131k verisi yay\u0131mlar. <b>\u00dc\u00e7 farkl\u0131 say\u0131, \u00fc\u00e7 farkl\u0131 anlam \u2014 her birini etiketleyin.<\/b><br \/><b>8. S\u00fctunlar\u0131 kaym\u0131\u015f da\u011f\u0131t\u0131mc\u0131 tablolar\u0131.<\/b> Yayg\u0131n olarak aynalanan bir B-3 PDF&#8217;inde akma <b>1370 MPa<\/b> (o, \u00b0C cinsinden solid\u00fcs), \u00e7ekme <b>216 MPa<\/b> (o, GPa cinsinden mod\u00fcl), genle\u015fme <b>50<\/b> (o, % uzama), sertlik <b>11,2 HRC<\/b> (o, \u0131s\u0131 iletkenli\u011fi) g\u00f6r\u00fcn\u00fcyor. <b>Akman\u0131n \u00e7ekmeyi a\u015ft\u0131\u011f\u0131 her tabloyu sa\u011fduyuyla kontrol edin.<\/b><br \/><b>9. Sertlik \u00f6l\u00e7e\u011fi kar\u0131\u015f\u0131kl\u0131\u011f\u0131.<\/b> B-3 <b>92\u201395 HRBW<\/b>&#8216;dir, kabaca <b>15\u201317 HRC<\/b>. &#8220;95&#8221;i HRC okuyan biri sa\u00e7ma bir sonuca var\u0131r. <b>\u00d6l\u00e7e\u011fi daima yaz\u0131n.<\/b><br \/><b>10. &#8220;B-3 gevrekle\u015fmeye ba\u011f\u0131\u015f\u0131kt\u0131r&#8221; \u2014 YANLI\u015e.<\/b> <b>Daha yava\u015ft\u0131r<\/b>: ~650 \u00b0C&#8217;de birka\u00e7 saat, B-2&#8217;nin dakikalar\u0131na kar\u015f\u0131; ve Ni\u2084Mo yerine Ni\u2083Mo olu\u015fturur. <b>H\u00e2l\u00e2 d\u00fczenlenme reaksiyonu olan bir Ni-Mo ala\u015f\u0131m\u0131d\u0131r.<\/b><\/p>\n<p><!-- \/dm-zengin --><\/p>\n<p><!-- dm-ld --><script type=\"application\/ld+json\">{\"@context\":\"https:\/\/schema.org\",\"@type\":\"WebPage\",\"name\":\"Hastelloy B-3\",\"url\":\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-b-3\/\",\"inLanguage\":\"tr\",\"description\":\"Hastelloy B-3 (UNS N10675 \/ W.Nr. 2.4600 \/ DIN NiMo29Cr), tek fazl\u0131 YMK (\u03b3) nikel-molibden kat\u0131 \u00e7\u00f6zelti ala\u015f\u0131m\u0131d\u0131r: nominal %65 Ni \u2013 %28,5 Mo, bilin\u00e7li olarak k\u00fc\u00e7\u00fck tutulmu\u015f Cr ve Fe, ve fiilen karbonsuz (C \u2264%0,010).\",\"isPartOf\":{\"@type\":\"WebSite\",\"name\":\"Defence Metal\",\"url\":\"https:\/\/www.defencemetal.com\/\"},\"publisher\":{\"@type\":\"Organization\",\"name\":\"Defence Metal\",\"url\":\"https:\/\/www.defencemetal.com\/\"},\"mainEntity\":{\"@type\":\"DefinedTerm\",\"name\":\"Hastelloy B-3\",\"description\":\"Hastelloy B-3 (UNS N10675 \/ W.Nr. 2.4600 \/ DIN NiMo29Cr), tek fazl\u0131 YMK (\u03b3) nikel-molibden kat\u0131 \u00e7\u00f6zelti ala\u015f\u0131m\u0131d\u0131r: nominal %65 Ni \u2013 %28,5 Mo, bilin\u00e7li olarak k\u00fc\u00e7\u00fck tutulmu\u015f Cr ve Fe, ve fiilen karbonsuz (C \u2264%0,010).\",\"inDefinedTermSet\":{\"@type\":\"DefinedTermSet\",\"name\":\"Defence Metal - metal ve ala\u015f\u0131mlar\",\"url\":\"https:\/\/www.defencemetal.com\/\"},\"alternateName\":[\"UNS N10675\",\"W.Nr. 2.4600\",\"NiMo29Cr\"],\"identifier\":[{\"@type\":\"PropertyValue\",\"propertyID\":\"UNS\",\"value\":\"N10675\"},{\"@type\":\"PropertyValue\",\"propertyID\":\"Werkstoffnummer\",\"value\":\"2.4600\"}],\"additionalProperty\":[{\"@type\":\"PropertyValue\",\"name\":\"DIN \/ EN ad\u0131\",\"value\":\"NiMo29Cr\"}]}}<\/script><!-- \/dm-ld --><\/p>\n","protected":false},"excerpt":{"rendered":"<p>Hastelloy B-3 \/ (2.4600) \/ UNS N10675 DEFENCE METAL Hastelloy B-3 UNS N10675 \u00b7 W.Nr. 2.4600 \u00b7 NiMo29Cr (DIN 17744) \u00b7 ISO NiMo30Cr \/ Ni1067 \u00b7 Ni %65,0 min \u2013 Mo %27,0-32,0 \u2013 Cr %1,0-3,0 \u2013 Fe %1,0-3,0 \u2013 Co %3,0 maks. \u2013 Mn %3,0 maks. \u2013 W %3,0 maks. \u2013 Al %0,50 maks. \u2013 &hellip; <\/p>\n<p class=\"link-more\"><a href=\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-b-3\/\" class=\"more-link\"><span class=\"screen-reader-text\"> &#8220;Hastelloy B-3&#8221;<\/span>devam\u0131n\u0131 oku<\/a><\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_yoast_wpseo_title":"Hastelloy B-3 \/ 2.4696 | UNS N10675 | Defence Metal","_yoast_wpseo_metadesc":"Hastelloy B-3 (W.Nr 2.4696, UNS N10675, NiMo29C) \u2014 \u00c7ubuk, lama, levha, sac, boru ve d\u00f6vme formlar\u0131nda temin edilir.","inspiro_hide_title":false,"inspiro_hide_featured_image":false,"footnotes":""},"dm_sektor":[10,13,15],"class_list":["post-830","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO plugin v28.5 - https:\/\/yoast.com\/product\/yoast-seo-wordpress\/ -->\n<title>Hastelloy B-3 \/ 2.4696 | UNS N10675 | Defence Metal<\/title>\n<meta name=\"description\" content=\"Hastelloy B-3 (W.Nr 2.4696, UNS N10675, NiMo29C) \u2014 \u00c7ubuk, lama, levha, sac, boru ve d\u00f6vme formlar\u0131nda temin edilir.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-b-3\/\" \/>\n<meta property=\"og:locale\" content=\"tr_TR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Hastelloy B-3 \/ 2.4696 | UNS N10675 | Defence Metal\" \/>\n<meta property=\"og:description\" content=\"Hastelloy B-3 (W.Nr 2.4696, UNS N10675, NiMo29C) \u2014 \u00c7ubuk, lama, levha, sac, boru ve d\u00f6vme formlar\u0131nda temin edilir.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/www.defencemetal.com\/index.php\/hastelloy-b-3\/\" \/>\n<meta property=\"og:site_name\" content=\"Defence Metal\" \/>\n<meta property=\"article:modified_time\" content=\"2026-09-25T13:26:25+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Tahmini okuma s\u00fcresi\" \/>\n\t<meta name=\"twitter:data1\" content=\"2 dakika\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/www.defencemetal.com\\\/index.php\\\/hastelloy-b-3\\\/\",\"url\":\"https:\\\/\\\/www.defencemetal.com\\\/index.php\\\/hastelloy-b-3\\\/\",\"name\":\"Hastelloy B-3 \\\/ 2.4696 | UNS N10675 | Defence Metal\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/www.defencemetal.com\\\/#website\"},\"datePublished\":\"2024-12-13T09:09:09+00:00\",\"dateModified\":\"2026-09-25T13:26:25+00:00\",\"description\":\"Hastelloy B-3 (W.Nr 2.4696, UNS N10675, NiMo29C) \u2014 \u00c7ubuk, lama, levha, sac, boru ve d\u00f6vme formlar\u0131nda temin edilir.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/www.defencemetal.com\\\/index.php\\\/hastelloy-b-3\\\/#breadcrumb\"},\"inLanguage\":\"tr\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/www.defencemetal.com\\\/index.php\\\/hastelloy-b-3\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/www.defencemetal.com\\\/index.php\\\/hastelloy-b-3\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Anasayfa\",\"item\":\"https:\\\/\\\/www.defencemetal.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Hastelloy B-3\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/www.defencemetal.com\\\/#website\",\"url\":\"https:\\\/\\\/www.defencemetal.com\\\/\",\"name\":\"Defence Metal\",\"description\":\"for better produce !\",\"publisher\":{\"@id\":\"https:\\\/\\\/www.defencemetal.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/www.defencemetal.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"tr\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/www.defencemetal.com\\\/#organization\",\"name\":\"Defence Metal\",\"url\":\"https:\\\/\\\/www.defencemetal.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"tr\",\"@id\":\"https:\\\/\\\/www.defencemetal.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/www.defencemetal.com\\\/wp-content\\\/uploads\\\/2024\\\/12\\\/cropped-logopngson.png\",\"contentUrl\":\"https:\\\/\\\/www.defencemetal.com\\\/wp-content\\\/uploads\\\/2024\\\/12\\\/cropped-logopngson.png\",\"width\":3846,\"height\":649,\"caption\":\"Defence Metal\"},\"image\":{\"@id\":\"https:\\\/\\\/www.defencemetal.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"http:\\\/\\\/www.linkedin.com\\\/company\\\/defencemetal\"],\"description\":\"Havac\u0131l\u0131k, savunma, enerji ve makine sekt\u00f6rleri i\u00e7in paslanmaz \u00e7elik, nikel ala\u015f\u0131mlar\u0131, titanyum, al\u00fcminyum ve ala\u015f\u0131ml\u0131 \u00e7elik tedarik eden \u00f6zel ala\u015f\u0131m tedarik\u00e7isi.\",\"email\":\"info@defencemetal.com\",\"telephone\":\"+90 216 709 74 41\",\"legalName\":\"Defence Metal\",\"address\":{\"@type\":\"PostalAddress\",\"streetAddress\":\"Cevizli Mah. Mustafa Kemal Cad. Hukuk\u00e7ular Towers A Blok No:66A \u0130\u00e7 Kap\u0131 No:111\",\"addressLocality\":\"Kartal\",\"addressRegion\":\"\u0130stanbul\",\"postalCode\":\"34865\",\"addressCountry\":\"TR\"},\"contactPoint\":{\"@type\":\"ContactPoint\",\"contactType\":\"sales\",\"telephone\":\"+90 216 709 74 41\",\"email\":\"info@defencemetal.com\",\"areaServed\":\"TR\",\"availableLanguage\":[\"Turkish\",\"English\"]}}]}<\/script>\n<!-- \/ Yoast SEO plugin. -->","yoast_head_json":{"title":"Hastelloy B-3 \/ 2.4696 | UNS N10675 | Defence Metal","description":"Hastelloy B-3 (W.Nr 2.4696, UNS N10675, NiMo29C) \u2014 \u00c7ubuk, lama, levha, sac, boru ve d\u00f6vme formlar\u0131nda temin edilir.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/www.defencemetal.com\/index.php\/hastelloy-b-3\/","og_locale":"tr_TR","og_type":"article","og_title":"Hastelloy B-3 \/ 2.4696 | UNS N10675 | Defence Metal","og_description":"Hastelloy B-3 (W.Nr 2.4696, UNS N10675, NiMo29C) \u2014 \u00c7ubuk, lama, levha, sac, boru ve d\u00f6vme formlar\u0131nda temin edilir.","og_url":"https:\/\/www.defencemetal.com\/index.php\/hastelloy-b-3\/","og_site_name":"Defence Metal","article_modified_time":"2026-09-25T13:26:25+00:00","twitter_card":"summary_large_image","twitter_misc":{"Tahmini okuma s\u00fcresi":"2 dakika"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"WebPage","@id":"https:\/\/www.defencemetal.com\/index.php\/hastelloy-b-3\/","url":"https:\/\/www.defencemetal.com\/index.php\/hastelloy-b-3\/","name":"Hastelloy B-3 \/ 2.4696 | UNS N10675 | Defence Metal","isPartOf":{"@id":"https:\/\/www.defencemetal.com\/#website"},"datePublished":"2024-12-13T09:09:09+00:00","dateModified":"2026-09-25T13:26:25+00:00","description":"Hastelloy B-3 (W.Nr 2.4696, UNS N10675, NiMo29C) \u2014 \u00c7ubuk, lama, levha, sac, boru ve d\u00f6vme formlar\u0131nda temin edilir.","breadcrumb":{"@id":"https:\/\/www.defencemetal.com\/index.php\/hastelloy-b-3\/#breadcrumb"},"inLanguage":"tr","potentialAction":[{"@type":"ReadAction","target":["https:\/\/www.defencemetal.com\/index.php\/hastelloy-b-3\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/www.defencemetal.com\/index.php\/hastelloy-b-3\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Anasayfa","item":"https:\/\/www.defencemetal.com\/"},{"@type":"ListItem","position":2,"name":"Hastelloy B-3"}]},{"@type":"WebSite","@id":"https:\/\/www.defencemetal.com\/#website","url":"https:\/\/www.defencemetal.com\/","name":"Defence Metal","description":"for better produce !","publisher":{"@id":"https:\/\/www.defencemetal.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/www.defencemetal.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"tr"},{"@type":"Organization","@id":"https:\/\/www.defencemetal.com\/#organization","name":"Defence Metal","url":"https:\/\/www.defencemetal.com\/","logo":{"@type":"ImageObject","inLanguage":"tr","@id":"https:\/\/www.defencemetal.com\/#\/schema\/logo\/image\/","url":"https:\/\/www.defencemetal.com\/wp-content\/uploads\/2024\/12\/cropped-logopngson.png","contentUrl":"https:\/\/www.defencemetal.com\/wp-content\/uploads\/2024\/12\/cropped-logopngson.png","width":3846,"height":649,"caption":"Defence Metal"},"image":{"@id":"https:\/\/www.defencemetal.com\/#\/schema\/logo\/image\/"},"sameAs":["http:\/\/www.linkedin.com\/company\/defencemetal"],"description":"Havac\u0131l\u0131k, savunma, enerji ve makine sekt\u00f6rleri i\u00e7in paslanmaz \u00e7elik, nikel ala\u015f\u0131mlar\u0131, titanyum, al\u00fcminyum ve ala\u015f\u0131ml\u0131 \u00e7elik tedarik eden \u00f6zel ala\u015f\u0131m tedarik\u00e7isi.","email":"info@defencemetal.com","telephone":"+90 216 709 74 41","legalName":"Defence Metal","address":{"@type":"PostalAddress","streetAddress":"Cevizli Mah. Mustafa Kemal Cad. Hukuk\u00e7ular Towers A Blok No:66A \u0130\u00e7 Kap\u0131 No:111","addressLocality":"Kartal","addressRegion":"\u0130stanbul","postalCode":"34865","addressCountry":"TR"},"contactPoint":{"@type":"ContactPoint","contactType":"sales","telephone":"+90 216 709 74 41","email":"info@defencemetal.com","areaServed":"TR","availableLanguage":["Turkish","English"]}}]}},"_links":{"self":[{"href":"https:\/\/www.defencemetal.com\/index.php\/wp-json\/wp\/v2\/pages\/830","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.defencemetal.com\/index.php\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/www.defencemetal.com\/index.php\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/www.defencemetal.com\/index.php\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/www.defencemetal.com\/index.php\/wp-json\/wp\/v2\/comments?post=830"}],"version-history":[{"count":22,"href":"https:\/\/www.defencemetal.com\/index.php\/wp-json\/wp\/v2\/pages\/830\/revisions"}],"predecessor-version":[{"id":6118,"href":"https:\/\/www.defencemetal.com\/index.php\/wp-json\/wp\/v2\/pages\/830\/revisions\/6118"}],"wp:attachment":[{"href":"https:\/\/www.defencemetal.com\/index.php\/wp-json\/wp\/v2\/media?parent=830"}],"wp:term":[{"taxonomy":"dm_sektor","embeddable":true,"href":"https:\/\/www.defencemetal.com\/index.php\/wp-json\/wp\/v2\/dm_sektor?post=830"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}